氢键型碳纳米管增强自修复复合材料的制备和表征

程尹杰 ,  张路 ,  胡仁杰 ,  王莹 ,  金学昕 ,  仇硕 ,  张颢严 ,  姜大伟

引用本文: 程尹杰, 张路, 胡仁杰, 王莹, 金学昕, 仇硕, 张颢严, 姜大伟. 氢键型碳纳米管增强自修复复合材料的制备和表征[J]. 应用化学, 2020, 37(10): 1147-1155. doi: 10.11944/j.issn.1000-0518.2020.10.200112 shu
Citation:  CHENG Yinjie, ZHANG Lu, HU Renjie, WANG Ying, JIN Xuexin, QIU Shuo, ZHANG Haoyan, JIANG Dawei. Preparation and Characterization of Hydrogen-Bonded Carbon Nanotubes Reinforced Self-healing Composites[J]. Chinese Journal of Applied Chemistry, 2020, 37(10): 1147-1155. doi: 10.11944/j.issn.1000-0518.2020.10.200112 shu

氢键型碳纳米管增强自修复复合材料的制备和表征

    通讯作者: 姜大伟, 讲师; Tel:0451-82135637;E-mail:sharkwei12345@163.com; 研究方向:自修复材料的设计和制备
  • 基金项目:

    央高校基本科研业务费专项资金项目(2572018BC27)、黑龙江省青年科学基金项目(QC2017038)、黑龙江省博士后特别资助(博士后青年英才计划)(LBH-TZ13)、黑龙江省政府博士后资助(LBH-Z16004)和中国博士后科学基金面上项目(2016M601402)资助

摘要: 使用低聚酸、二乙烯三胺以及尿素为原料,碳纳米管为增强剂,制备出兼具良好力学性能和室温(30℃)自修复性能的氢键型自修复复合材料,同时对材料通过氢键进行自修复的机制进行了合理推测。首先,对不同碳纳米管添加量的自修复材料进行应力-应变性能测试。结果发现,随着碳纳米管的添加,材料的应力、应变均有所提高,添加质量分数9%碳纳米管时,材料的应力达到4.1 MPa、应变达到6%以上。对添加质量分数9%碳纳米管的自修复材料进行表面形态、自修复性能以及热稳定性能测试。结果表明,碳纳米管与材料有良好的相容性,材料的表面与切面形态相似;在室温下自修复24 h,自修复效率达到100%;10次断裂-修复循环中自修复效率仍能保持90%以上;材料具有良好的热稳定性,最大失重速率下的温度为474.3℃。为下一代类皮肤传感器以及可穿戴智能设备提供了一种选择,为未来该类型自修复聚合物复合材料在高拉伸强度领域的应用奠定了技术基础。

English

  • “自修复”是一个来自于仿生学的概念。当生物体遭受创伤后其组织可进行自我修复并恢复其原有功能。近几年这种具有自我修复功能的智能材料[1]已被应用于机器人电子皮肤[2]、柔性传感器[3]、可拉伸储能设备[4]以及柔性屏幕和生物医疗[5]等领域。构建自修复材料的策略通常分为两种:1)外援型自修复,即在材料的制备过程中将修复剂以微胶囊或微脉管的形式添加到材料中,当材料受损,微胶囊或微脉管破裂,修复剂流出,像粘合剂一样将受损材料粘接起来[6];2)本征型自修复,即通过材料本身存在的动态非共价键或可逆化学反应进行的自修复[7]。尽管外援型自修复技术成熟、修复效率高,但其修复次数有限而且需要外加修复剂,微胶囊或微脉管的引入也会削弱材料本身的力学性能,不适用于非常薄的材料,例如智能电子皮肤。本征型自修复材料由于可多次重复修复,具有良好的可拉伸性能,更接近于“智能材料”,因此引起了更多科学家的关注。本征型修复是利用聚合物材料中的可逆化学反应,如Diels-Alder反应[8]、金属配位键[9-10]、双硫键反应[11-12]或动态非共价键作用,如π-π堆叠[13]和氢键等进行的自修复。可逆酰腙键和双硫键自修复对pH值比较敏感,无法适应大多数pH值恒定的场合。而可逆N—O键自修复对温度要求比较严格,修复时间较长,因此无法满足温度变化较大的场合。可逆Dieal-Alder反应容易进行,且反应速率快,但需加热才能完成修复[14]。

    氢键作为常见的动态非共价键,被广泛地应用在本征型自修复聚合物领域。Kang等[15]使用双(3-氨基丙基)封端的聚二甲基硅氧烷(H2N-PDMS-NH2, Mn=5000)与4, 4-亚甲基双(苯基异氰酸酯)和异泊酮二异氰酸酯反应合成了一种具有强弱两种氢键的自修复聚合物。强交联氢键使自修复聚合物坚固具有弹性,弱交联氢键通过有效的可逆断裂和变形来消耗应变能,降低了材料对破损的敏感性,使材料拥有出色的自修复效率。尽管动态氢键赋予聚合物良好的自修复性能,但过少的氢键无法提供良好的自修复性能,而过多的氢键又抑制了聚合物链之间的移动,增加材料的韧性同时也削弱了材料在室温下的自修复能力。如Cordier等[16]使用低聚酸和二乙烯三胺制备了一种基于氢键的自修复聚合物。该聚合物在较高温度下展现出了良好的自修复性能,但其室温修复性能以及力学性能较差。

    碳纳米管[17](CNTs)是卷曲成圆柱状的片层石墨烯,通常直径可达100 nm而长度为微米级别。其拉伸强度可达50~100 GPa,弯曲强度可达14.2 GPa。并且由于其中空结构可通过改变体积实现弹性形变,而不会出现断裂的情况,因此最大弯曲角度超过110°。出色的力学性能使CNTs成为制备高性能聚合物纳米复合材料的理想增强体[18]。1994年,Ajayan[19]首次报道了CNTs增强聚合物纳米复合材料。此后有大量的研究证实了CNTs对聚合物的增强作用,其中包括在聚乙烯[20-21]、环氧树脂[22-23]、聚酰亚胺[24]以及聚氨酯[25]等体系。但对于CNTs增强聚合物而言,最大的问题在于如何使CNTs有效地分散在聚合物基质中[26]。常规的CNTs分散方法有溶液混合、熔融混合、静电纺丝、原位聚合以及CNTs的化学官能化等。其中,CNTs的化学官能化[27]是一种简单有效的防止CNTs团聚、提高分散度的方法。Kuan等[28]报道了胺基官能化CNTs对聚氨酯的增强作用。添加胺基化CNTs的聚氨酯相比于未添加CNTs的聚氨酯,模量增加了70%。羧基化的CNTs作为一种增强剂,应用于富含氢键的聚合物体系,提高了聚合物的力学性能[29-30]。但官能化CNTs应用于自修复聚合物中还鲜见报道[31]。

    制备具有高机械强度且同时具有优良室温修复性能的自修复聚合物仍然具有挑战。因此, 本文在多重氢键自修复聚合物的基础上添加分散性较好的羟基化CNTs作为增强剂,制备了一系列CNTs增强的自修复酰胺聚合物材料,在保持氢键数量的同时,增强了材料机械强度,比较了CNTs增强前后材料的力学性能、自修复性能、表面形态以及热稳定性能,并对自修复机制进行了理论推测。

    低聚酸(分析纯)购自上海高鸣化工有限公司;二乙烯三胺(分析纯)购自上海迈瑞尔化学技术有限公司;羟基化多壁碳纳米管(MWCNTs-OH)(试剂级)购自苏州碳丰石墨烯科技有限公司;氯仿、甲醇、尿素、乙醇、丙酮均购自天津市天力化学试剂有限公司,均为分析纯试剂。

    WDW-2型微机控制电子万能试验机(济南永科试验仪器有限公司);Pyris1型热重分析仪(TGA,美国PE公司);SU8020型扫描电子显微镜(SEM,日本Hitachi公司)。

    1.2.1   低聚物的制备

    低聚物的合成参考文献[32]中的方法。首先,将30 g低聚酸与12.3 g二乙烯三胺在N2气氛围下,搅拌加热到160 ℃并保持24 h。停止加热,冷却到室温,得到低聚物粗产品。粗产品使用50 mL氯仿洗涤3次,再加入90 mL乙醇和水的混合液(体积比1:2)洗涤后得到低聚物。

    1.2.2   自修复聚合物的制备

    本实验参考文献[15]中的合成方法进行CNTs增强自修复聚合物复合材料的系列制备。具体步骤如下:称取5 g低聚物、1.18 g尿素于装有回流冷凝管的100 mL三口烧瓶中,分别添加0.00、0.15、0.25、0.35、0.45 g碳纳米管,机械搅拌,N2气保护。加热至135 ℃后,控制加热速度为5 ℃/h,待反应体系温度升高至160 ℃时,保持1.5 h,停止反应。得到CNTs增强自修复聚合物复合材料,分别表示为0%CNTs、3%CNTs、5%CNTs、7%CNTs、9%CNTs。将生成的自修复材料放在聚四氟乙烯片上,置于干燥器中保存。制备流程如图 1所示。

    图 1

    图 1.  自修复聚合物的制备流程图
    Figure 1.  Schematic diagram of preparation of the self-repairing polymer
    1.2.3   测试样品的制备

    将制备的自修复聚合物放置于定制的聚四氟乙烯模板中,设置气动压机压力为0.2 MPa、温度为90 ℃对材料进行压制。得到30 mm×7 mm×1 mm的测试样品。将样品放置于干燥器内,干燥,备用。

    1.3.1   力学性能测试

    对制备的不同CNTs含量的样品进行拉伸性能测试,拉伸速度为1 mm/min。筛选出力学性能最佳的CNTs增强自修复聚合物复合材料,进行后续测试。

    1.3.2   SEM测试

    使用SEM观察力学性能最佳的样品表面以及断裂修复后表面的微观形貌。

    1.3.3   热重分析

    测试过程中使用N2气气氛,升温速度10 ℃/min,温度范围50~800 ℃。

    1.3.4   自修复性能测试

    在220 V、50 Hz、1 kW条件下,以1 mm/min的速率进行力学拉伸性能测试试验,将样品拉伸断裂后让断裂处重新接触,将样品分别置于30、40、50和60 ℃下分别修复1、2、3、6和24 h。然后,再进行力学性能测试。通过系列修复性能测试确定最佳修复条件。在最佳修复条件下,进行10次拉伸-断裂-修复循环测试,测试其修复效率。

    所制得的CNTs增强复合材料的应力-应变曲线如图 2所示,材料的拉伸强度如图 3所示。可以看出,不添加CNTs的复合材料拉伸应变为0,在应力为0.7 MPa时就彻底断裂。添加CNTs之后材料的应力应变均有明显的增加,当添加的CNTs质量分数为9%时,材料的应力可达到4.1 MPa,应变达到6%以上。

    图 2

    图 2.  CNTs增强复合材料的应力-应变曲线
    Figure 2.  The stress-strain curves of the composites enhanced by carbon nanotubes

    图 3

    图 3.  不同CNTs添加比例的材料拉伸强度
    Figure 3.  Tensile strength of materials with different proportions of CNTs

    CNTs对材料的力学性能有明显的增强作用,原因是材料本身是体积较大、结构对称性较低的二元酸和三元酸与二乙烯三胺聚合形成的低聚物(如图 1所示),虽然分子中存在大量N—H、O—H、C=O键,使得分子之间存在很强的氢键作用,但是分子中的环状结构和环上所连较长脂肪链,氢键的形成,阻碍了分子的运动,使得材料变脆,力学性能很差。而CNTs,实际上使用的是MWCNTs,结构中存在大量—OH和—COOH,这些基团可以和聚合物分子中的N—H、O—H、C=O键形成氢键,分散了聚合物分子之间的直接作用力,就像一道道桥梁,将聚合物分子连接起来,即增加了分子的运动灵活性,又提高了聚合物分子之间的接触作用力,增强了材料的力学性能。起初,随着CNTs的添加量增大,这种桥梁作用也来越强。但是当CNTs的添加达到一定量,CNTs之间容易发生团聚,增加了聚合物分子间距离,阻断聚合物分子间的连接,使材料难以成型。当CNTs质量分数超过9%之后,材料就不易成型了。因此,选择添加质量分数9%的CNTs的样品作为后续测试。

    图 4为质量分数9%CNTs复合材料的自修复过程的实物展示图。当断面重新接触后修复过程即可自发进行,修复完成后表面平整无明显裂纹。修复后的材料可承受2个200 g砝码而不发生断裂。

    图 4

    图 4.  自修复过程的实物展示图(A)材料被切割;(B)材料断裂;(C)将断面接触到一起;(D)材料自我修复;(E)材料修复后可悬挂2个200 g砝码
    Figure 4.  Photographs of the self-healing process (A) material being cut; (B) fractured material; (C) contact of sections together; (D) material self-healing; (E) two 200 g weights can be suspended after material healing

    修复效率(η)通过下式进行计算。

    $ \eta = {G_1}/{G_0} $

    (1)

    式中,G1为样品修复后的断裂拉伸强度(MPa),G0为样品原始的断裂拉伸强度(MPa)。

    不同修复温度、不同修复时间下,材料的自修复效率如图 5所示。随着自修复时间增加,材料的自修复效率明显提高,自修复24 h的自修复效率在室温以上均达到100%。而且室温下自修复24 h的材料,可以轻松承受400 g(571 kg/m2)的重物。随着修复温度增加,自修复效率也有所增加。室温下修复1 h,修复效率35%;60 ℃下修复1 h,修复效率提高到55%。60 ℃下修复6 h,自修复效率就可以达到100%。这是由于温度高于材料的玻璃化转变温度时,材料的性质更接近于橡胶,有助于自修复进程。因此,选择60 ℃下自修复6 h这一较优自修复条件,对材料在60 ℃下进行10次拉伸-断裂-自修复的循环自修复性能测试,结果如图 6所示。结果表明,在60 ℃自修复6 h条件下,自修复聚合物在10次拉伸-断裂-自修复循环测试后,自修复效率仍能保持在90%以上。

    图 5

    图 5.  CNTs增强自修复聚合物材料在不同温度下的修复效率
    Figure 5.  Self-healing efficiencies of CNTs reinforced self-healing composites materials at different temperatures

    图 6

    图 6.  在60 ℃自修复6 h条件下, 材料的循环修复性能
    Figure 6.  Healing cycles properties of materials at 60 ℃ for 6 h healing

    图 7为材料表面、切断面以及自修复后表面的SEM图片。可见,质量分数9%CNTs材料的表面光滑平整,看不出CNTs存在的迹象,说明CNTs与聚合物基材相容性很好。因为CNTs是羟基化的,表面含有羟基和羧基,与聚合物的极性基团可以形成偶极作用和氢键作用,形成相容体系。切开的质量分数9%CNTs材料切面与材料的表面看起来十分相似,当两个切面重新靠在一起,切面之间的分子重新形成氢键,发生自修复,切开的两段重新融合在一起,如图 7C所示。

    图 7

    图 7.  9%CNTs复合材料表面(A)、截面(B)和自修复表面(C)的扫描电子显微镜图像
    Figure 7.  Scanning electron microscopy images of 9%CNTs composites for (A) material surface (B) material incision section (C) self-healing surface

    通过两步法合成自修复聚合物。使用常见的天然可再生资源脂肪低聚酸为原料,第1步将其与二乙烯三胺进行聚合反应生成多重羧基封端的低聚物,低聚物分子之间应该存在强烈的氢键作用。

    通常简单的二元酸与二乙烯三胺发生反应生成线性结构,线性结构有利于结晶,这对自修复很不利。本文采用二元酸与三元酸的混合体系,由于混合熵的存在有效地避免了结晶。由于第1步中酸添加过量,在第2步加入尿素后尿素继续与酸官能团反应,生成了氨基乙基咪唑酮(Ⅰ)、二(氨基乙基)脲(Ⅱ)、二氨基四乙基三脲(Ⅲ)等多种含有互补氢键官能团的低聚物混合物,如图 8所示。其中—C=O双键为氢键受体,—N—H键为氢键供体,这些官能团之间可以形成多重氢键作用,形成超分子网络。但是,氢键的形成,阻碍了体积较大、对称性较差的聚合物分子运动,所以材料较脆,容易断裂,应力和应变较低,最终得到的产物为半透明脆性的固体。为了进一步提升材料的机械强度,使用羟基化CNTs作为增强剂。羟基化CNTs富含羟基和羧基,通过氢键作用,像桥梁一样将聚合物分子连接起来,与聚合物材料发生作用(如图 8所示),同时,降低聚合物分子间的氢键作用、促进了聚合物分子的运动能力,从而提高了材料的应力、应变和拉伸强度。

    图 8

    图 8.  (A) 二元酸,二乙烯三胺与尿素反应过程中生成的3种官能团,Ⅰ:氨基乙基咪唑酮,Ⅱ:二(氨基乙基)脲,Ⅲ:二氨基四乙基三脲;(B)3种官能团以及羟基化CNTs之间形成的可逆氢键;(C)羟基化碳纳米管的结构示意图
    Figure 8.  (A) Three functional groups formed during the reaction of diacid, diethylenetriamine and urea, among which Ⅰ:aminoethylimidazolone, Ⅱ:di(aminoethylurea) urea, Ⅲ:diaminotetraethyl triurea. (B) Reversible hydrogen bonds formed between three functional groups and hydroxylated CNTs. (C) Schematic diagram of hydroxylated carbon nanotubes

    开裂材料的自修复过程如图 9所示。受外力作用,材料开裂,可逆的动态非化学键作用—氢键随即断开。但是形成氢键的位点还存在着,当裂口断面相接触,氢键重新形成,使材料愈合,完成自修复。

    图 9

    图 9.  材料在断裂-修复过程中氢键的断裂与形成
    Figure 9.  The fracture and formation of hydrogen bonds during the fracture and repair process of the material

    质量分数0%CNTs和质量分数9%CNTs自修复材料的TG/DTG结果如图 10所示。可见,质量分数9%CNTs自修复材料与质量分数0%CNTs失重趋势很接近,二者热稳定性均很高,CNTs增强的自修复材料热稳定性更高一些,最大失重速率下的温度由未添加CNTs的450.1 ℃升高到474.3 ℃。700 ℃下的残留量由1.4%提高到7.3%。也就是说,CNTs的添加,提高了自修复材料的热稳定性,减少了热分解量。

    图 10

    图 10.  自修复聚合物TG/DTG曲线
    Figure 10.  TG/DTG curves of the self-healing polymers

    表 1

    表 1  自修复材料的热重分析特征数据表
    Table 1.  TG analysis of self-healing materials
    下载: 导出CSV
    Sample Tmax/℃ Vmax/(%·min-1) R700/%
    9%CNTs 474.3 -13.3 7.3
    0%CNTs 450.1 -10.6 1.4
      Notes:Tmax is the maximum decomposition temperature; Vmax is the maximum mass loss rate; R700 is the residual amount at 700 ℃.

    本文用羟基化碳纳米管(CNTs)作增强剂制备了氢键型室温自修复复合材料。羟基化CNTs能均匀地分散在聚合物基质中,加入羟基化CNTs后材料展现出更加优异的力学性能以及热稳定性。该材料在室温到60 ℃范围内均可以展现出良好的自修复性能,并且修复性能展现出良好的可重复性,在10次的修复循环后修复效率仍保持90%以上。这主要是由于材料中存在的多重氢键。这种出色的拉伸强度、韧性以及自修复特性也为未来研发柔性电子设备提供了多种可能性。这种可伸缩和整合的电子设备将在新兴的仿生机器人和可穿戴医疗设备中实现诸多应用,但这仍是一个漫长且复杂的过程,尤其需要材料学、生物科学以及电子技术等多学科的交叉研究。


    1. [1]

      Guimard N K, Oehlenschlaeger K K, Zhou J. Current Trends in the Field of Self-healing Materials[J]. Macromol Chem Phys, 2012, 213(2):  131-143. doi: 10.1002/macp.201100442

    2. [2]

      Cheng K, Huang C, Wei Y. Novel Chitosan-Cellulose Nanofiber Self-healing Hydrogels to Correlate Self-healing Properties of Hydrogels with Neural Regeneration Effects[J]. NPG Asia Mater, 2019, 11(1):  25. doi: 10.1038/s41427-019-0124-z

    3. [3]

      Lei Z, Wang Q, Sun S. A Bioinspired Mineral Hydrogel as a Self-healable, Mechanically Adaptable Ionic Skin for Highly Sensitive Pressure Sensing[J]. Adv Mater, 2017, 29(22):  1700321. doi: 10.1002/adma.201700321

    4. [4]

      Dubal D P, Chodankar N R, Kim D. Towards Flexible Solid-State Supercapacitors for Smart and Wearable Electronics[J]. Chem Soc Rev, 2018, 47(6):  2065-2129. doi: 10.1039/C7CS00505A

    5. [5]

      Chen J, Huang Y, Ma X. Functional Self-Healing Materials and Their Potential Applications in Biomedical Engineering[J]. Adv Compos Hybrid Mater, 2017, 11:  1-20.

    6. [6]

      Mcdonald S A, Coban S B, Sottos N R. Tracking Capsule Activation and Crack Healing in a Microcapsule-Based Self-healing Polymer[J]. Sci Rep, 2019, 9(1):  17773. doi: 10.1038/s41598-019-54242-7

    7. [7]

      Wang Y, Jiang D, Zhang L. Hydrogen Bonding Derived Self-healing Polymer Composites Reinforced with Amidation Carbon Fibers[J]. Nanotechnology, 2020, 31(2):  25704. doi: 10.1088/1361-6528/ab4743

    8. [8]

      Macedo L G, Orozco F, Picchioni F. Electrically Self-Healing Thermoset MWCNTs Composites Based on Diels-Alder and Hydrogen Bonds[J]. Polymers, 2019, 11(11):  1885. doi: 10.3390/polym11111885

    9. [9]

      Li C H, Zuo J L. Self-healing Polymers Based on Coordination Bonds[J]. Adv Mater, 2020, 32:  1903762.

    10. [10]

      Wang Z, Xie C, Yu C. A Facile Strategy for Self-healing Polyurethanes Containing Multiple Metal-Ligand Bonds[J]. Macromol Rapid Commun, 2018, 39(6):  1700678. doi: 10.1002/marc.201700678

    11. [11]

      Chang K, Jia H, Gu S. A transparent, Highly Stretchable, Self-healing Polyurethane Based on Disulfide Bonds[J]. Eur Polym J, 2019, 112:  822-831. doi: 10.1016/j.eurpolymj.2018.11.005

    12. [12]

      Wang Y, Li Y, Bai J. A Robust and High Self-healing Efficiency Poly(Urea-Urethane) Based on Disulfide Bonds with Cost-Effective Strategy[J]. Macromol Chem Phys, 2019, :  1900340.

    13. [13]

      Debroy S, Pavan Kumar Miriyala V, Vijaya Sekhar K. Self Healing Nature of Bilayer Graphene[J]. Superlattices Microstruct, 2016, 96:  26-35. doi: 10.1016/j.spmi.2016.05.010

    14. [14]

      Li S, Wang L, Yu X. Synthesis and Characterization of a Novel Double Cross-linked Hydrogel Based on Diels-Alder Click Reaction and Coordination Bonding[J]. Mater Sci Eng C, 2018, 82:  299-309. doi: 10.1016/j.msec.2017.08.031

    15. [15]

      Kang J, Son D, Wang G N. Tough and Water-Insensitive Self-healing Elastomer for Robust Electronic Skin[J]. Adv Mater, 2018, 30(13):  1706846. doi: 10.1002/adma.201706846

    16. [16]

      Cordier P, Tournilhac F, Soulie-Ziakovic C. Self-healing and Thermoreversible Rubber from Supramolecular Assembly[J]. Nature, 2008, 451(7181):  977-980. doi: 10.1038/nature06669

    17. [17]

      Rao C N, Satishkumar B C, Govindaraj A. Nanotubes[J]. Chemphyschem, 2001, 2(2):  78-105. doi: 10.1002/1439-7641(20010216)2:2<78::AID-CPHC78>3.0.CO;2-7

    18. [18]

      Siddons G P, Merchin D, Back J H. Highly Efficient Gating and Doping of Carbon Nanotubes with Polymer Electrolytes[J]. Nano Lett, 2004, 4(5):  927-931. doi: 10.1021/nl049612y

    19. [19]

      Ajayan P M, Stephan O, Colliex C. Aligned Carbon Nanotube Arrays Formed by Cutting a Polymer Resin-Nanotube Composite[J]. Science, 1994, 265(5176):  1212-1214. doi: 10.1126/science.265.5176.1212

    20. [20]

      Hsiao A, Tsai S, Hsu M. Decoration of Multi-Walled Carbon Nanotubes by Polymer Wrapping and Its Application in MWCNT/Polyethylene Composites[J]. Nanoscale Res Lett, 2012, 7(40):  1-5.

    21. [21]

      Aguiar V O, Pita V J R R, Marques M D F V. Nanocomposites of Ultrahigh Molar Mass Polyethylene and Modified Carbon Nanotubes[J]. J Appl Polym Sci, 2019, 136(19):  47459. doi: 10.1002/app.47459

    22. [22]

      Shen L, Liu L, Wu Z. Tensile Mechanical Behaviors of High Loading of Carbon Nanotube/Epoxy Composites via Experimental and Finite Element Analysis[J]. Adv Eng Mater, 2019, :  1900895.

    23. [23]

      Isarn I, Bonnaud L, Massagues L. Study of the Synergistic Effect of Boron Nitride and Carbon Nanotubes in the Improvement of Thermal Conductivity of Epoxy Composites[J]. Polym Int, 2020, 69(3):  280-290. doi: 10.1002/pi.5949

    24. [24]

      Yuen S, Ma C M, Chiang C. Preparation and Morphological, Electrical, and Mechanical Properties of Polyimide-Grafted MWCNT/Polyimide Composite[J]. J Polym Sci Pol Chem, 2007, 45(15):  3349-3358. doi: 10.1002/pola.22085

    25. [25]

      Lee C, Liu J, Chen S. Miscibility and Properties of Acid-Treated Multi-walled Carbon Nanotubes/Polyurethane Nanocomposites[J]. Polym J, 2007, 39(2):  138-146.

    26. [26]

      Sahoo N G, Rana S, Cho J W. Polymer Nanocomposites Based on Functionalized Carbon Nanotubes[J]. Prog Polym Sci, 2010, 35(7):  837-867. doi: 10.1016/j.progpolymsci.2010.03.002

    27. [27]

      Hirsch A. Functionalization of Single-walled Carbon Nanotubes[J]. Angew Chem, 2002, 41(11):  1853-1859. doi: 10.1002/1521-3773(20020603)41:11<1853::AID-ANIE1853>3.0.CO;2-N

    28. [28]

      Kuan H C, Ma C, Chang W P. Synthesis, Thermal, Mechanical and Rheological Properties of Multiwall Carbon Nano Tube/Waterborne Polyurethane Nanocomposite[J]. Compos Sci Technol, 2005, 65(11/12):  1703-1710.

    29. [29]

      Sahoo N G, Jung Y C, Yoo H J. Influence of Carbon Nanotubes and Polypyrrole on the Thermal, Mechanical and Electroactive Shape-Memory Properties of Polyurethane Nanocomposites[J]. Compos Sci Technol, 2007, 67(9):  1920-1929. doi: 10.1016/j.compscitech.2006.10.013

    30. [30]

      Sahoo N G, Jung Y C, Yoo H J. Effect of Functionalized Carbon Nanotubes on Molecular Interaction and Properties of Polyurethane Composites[J]. Macromol Chem Phys, 2006, 207(19):  1773-1780. doi: 10.1002/macp.200600266

    31. [31]

      Marialuigia R, Carlo N, Luigi V. Multifunctionality of Structural Nanohybrids:The Crucial Role of Carbon Nanotube Covalent and Non-Covalent Functionalization in Enabling High Thermal, Mechanical and Self-healing Performance[J]. Nanotechnology, 2020, 31(22):  225708. doi: 10.1088/1361-6528/ab7678

    32. [32]

      Xing L, Li Q, Zhang G. Self-healable Polymer Nanocomposites Capable of Simultaneously Recovering Multiple Functionalities[J]. Adv Funct Mater, 2016, 26(20):  3524-3531. doi: 10.1002/adfm.201505305

  • 图 1  自修复聚合物的制备流程图

    Figure 1  Schematic diagram of preparation of the self-repairing polymer

    图 2  CNTs增强复合材料的应力-应变曲线

    Figure 2  The stress-strain curves of the composites enhanced by carbon nanotubes

    图 3  不同CNTs添加比例的材料拉伸强度

    Figure 3  Tensile strength of materials with different proportions of CNTs

    图 4  自修复过程的实物展示图(A)材料被切割;(B)材料断裂;(C)将断面接触到一起;(D)材料自我修复;(E)材料修复后可悬挂2个200 g砝码

    Figure 4  Photographs of the self-healing process (A) material being cut; (B) fractured material; (C) contact of sections together; (D) material self-healing; (E) two 200 g weights can be suspended after material healing

    图 5  CNTs增强自修复聚合物材料在不同温度下的修复效率

    Figure 5  Self-healing efficiencies of CNTs reinforced self-healing composites materials at different temperatures

    图 6  在60 ℃自修复6 h条件下, 材料的循环修复性能

    Figure 6  Healing cycles properties of materials at 60 ℃ for 6 h healing

    图 7  9%CNTs复合材料表面(A)、截面(B)和自修复表面(C)的扫描电子显微镜图像

    Figure 7  Scanning electron microscopy images of 9%CNTs composites for (A) material surface (B) material incision section (C) self-healing surface

    图 8  (A) 二元酸,二乙烯三胺与尿素反应过程中生成的3种官能团,Ⅰ:氨基乙基咪唑酮,Ⅱ:二(氨基乙基)脲,Ⅲ:二氨基四乙基三脲;(B)3种官能团以及羟基化CNTs之间形成的可逆氢键;(C)羟基化碳纳米管的结构示意图

    Figure 8  (A) Three functional groups formed during the reaction of diacid, diethylenetriamine and urea, among which Ⅰ:aminoethylimidazolone, Ⅱ:di(aminoethylurea) urea, Ⅲ:diaminotetraethyl triurea. (B) Reversible hydrogen bonds formed between three functional groups and hydroxylated CNTs. (C) Schematic diagram of hydroxylated carbon nanotubes

    图 9  材料在断裂-修复过程中氢键的断裂与形成

    Figure 9  The fracture and formation of hydrogen bonds during the fracture and repair process of the material

    图 10  自修复聚合物TG/DTG曲线

    Figure 10  TG/DTG curves of the self-healing polymers

    表 1  自修复材料的热重分析特征数据表

    Table 1.  TG analysis of self-healing materials

    Sample Tmax/℃ Vmax/(%·min-1) R700/%
    9%CNTs 474.3 -13.3 7.3
    0%CNTs 450.1 -10.6 1.4
      Notes:Tmax is the maximum decomposition temperature; Vmax is the maximum mass loss rate; R700 is the residual amount at 700 ℃.
    下载: 导出CSV
  • 加载中
计量
  • PDF下载量:  10
  • 文章访问数:  2480
  • HTML全文浏览量:  445
文章相关
  • 发布日期:  2020-10-01
  • 收稿日期:  2020-04-19
  • 接受日期:  2020-07-20
  • 修回日期:  2020-06-22
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

/

返回文章