Strain engineering of heterogeneous catalysts for oxygen reduction reaction

Yuan Zhao ,  Hanqi Yu ,  Jiuchao Tang ,  Yingmei Li ,  Xue Yong ,  Xin Tu ,  Jing Wang

Citation:  Yuan Zhao, Hanqi Yu, Jiuchao Tang, Yingmei Li, Xue Yong, Xin Tu, Jing Wang. Strain engineering of heterogeneous catalysts for oxygen reduction reaction[J]. Chinese Chemical Letters, 2027, 38(1): 111997. doi: 10.1016/j.cclet.2025.111997 shu

Strain engineering of heterogeneous catalysts for oxygen reduction reaction

English

  • Reducing the dependence on fossil fuels to minimize human activity induced environmental pollution and resources depletion is an indispensable commitment, which requires innovation in clean and renewable energy at low cost [1-10]. Within sustainable energy frameworks, the oxygen reduction reaction (ORR) represents a cornerstone of electrochemical research, serving as a fundamental mechanism for developing next-generation energy storage devices including fuel cells and advanced battery systems [11-21]. Current technological limitations stem from inadequate catalytic performance in existing materials, particularly regarding reaction rate optimization and operational stability [22,23]. Heterogeneous catalysts play a crucial role in the ORR process, as they not only enhance the reaction kinetics but also facilitate the efficient separation from products, demonstrating improved durability [24-29]. Precious metal catalysts, such as platinum (Pt), exhibits high activity and has been mainly applied in the commercial market, however, the high cost, limited availability, and impressionable conditions are significant barriers to their widespread application [30,31]. Meanwhile, transition metal catalysts have been extensively investigated as potential substitutes for noble metal counterparts. Nevertheless, their catalytic performance in terms of reaction efficiency and product specificity frequently encounters fundamental limitations arising from unavoidable thermodynamic constraints and kinetic challenges embedded within catalytic mechanisms [32-34].

    Strain engineering has emerged as a promising strategy to enhance the catalytic performance of heterogeneous catalysts [35-39]. Inducing tensile and compressive strains in catalytic materials can modulate the electronic structure, active site distribution, and adsorption energies of reactants and intermediates, which enables to optimize reaction kinetics precisely in nanoscale [40-42]. Within ORR systems, strain engineering improves catalytic efficiency via multiple pathways. The strategic introduction of strain alters transition metals' d-band center positioning, thereby regulating intermediate species' adsorption energies. For example, controlled lattice distortions can strengthen oxygen-containing compound binding through optimized interatomic spacing and angular configurations, significantly accelerating reaction sequences [43]. Moreover, the introduction of defects or the use of heterostructures induced strain can create localized regions of high reactivity that preferentially stabilize reaction intermediates, effectively lowering the energy barriers associated with the ORR [44,45]. Additionally, the interactions between different phases in the composites can also contribute to strain-induced effects that bolster catalytic efficiency. To date, numerous studies have been published on strain engineering and the modulation of ORR catalysts. For instance, Wang et al. [46] found that under the drive of surface stress, two-dimensional transition metal nanosheets generate an intrinsic strain, and controlling the thickness of the material at atomic scale can realize the regulation of the intrinsic strain, for example, compared with Pd nanoparticles, the 5-layer thickness Pd nanosheets showed 1.2% compressive strain and 50 times more ORR activity than the nanoparticles. Yu et al. [47] synthesized a zig-zag ultrafine Pt nanowires catalyst, whose surface stress released by abundant low-coordinated atoms on the surface improved the specific activity (SA) and mass activity (MA) of the fuel cell catalyst. Zeng et al. [48] extended the research to the surface containing step defects, and confirmed that the surface defects or heteroatom deposition of Pt (111) step surface will cause surface stress release, driving the surface to produce non-uniform strain field, resulting in highly local changes in surface electronic structure and adsorption energy and altering the activity of specific sites by orders of magnitude. These examples demonstrate the flexibility and effectiveness of strain engineering to precisely modulate the electronic structure and activity of catalysts, providing an important strategy for designing well-performed electrocatalysts. Yet, there remains a conspicuous absence of a systematic and comprehensive review that provides an in-depth exploration of the strain engineering in the development of heterogeneous catalysts for the ORR.

    In this review, it is aimed to describe the current progress of strain engineering applied to heterogeneous catalysts for ORR, from the aspects of the theoretical insights, experimental methods and recent breakthroughs. It starts with a discussion on the fundamental principles of ORR and strain engineering, followed by a detailed examination of the six strategies employed to induce strain in catalytic materials (Fig. 1). Subsequently, it is delved into a series of case studies that illustrate the impact of strain engineering on the performance of different types of catalysts, including both precious and non-precious metal systems. Finally, it is concluded with perspectives on future research directions and the potential challenges that must be addressed to fully leverage the benefits of strain engineering in the quest for demanded electrocatalysts. It is aimed to establish transformative ideas and theoretical foundation for the rational design of ORR electrocatalysts, which may also be illuminate for other green energy related reactions.

    Figure 1

    Figure 1.  Schematic diagram of strain engineering and ORR catalysts.

    The efficiency of ORR primarily centers on breaking the O=O double bond in oxygen molecules followed by hydrogenation reduction processes [49]. This electrochemical reaction proceeds via either 2e− or 4e− transfer pathways (Fig. 2). The 4e− route encompasses both dissociative and associative electrochemical routes. In the dissociative pathway, molecular oxygen typically adsorbs across dual active sites forming a bridged oxygen configuration that subsequently undergoes cleavage to generate *O species. Conversely, the associative mechanism involves end-on oxygen adsorption at single active sites, followed by protonation to create *OOH intermediates. The acid-mediated dissociative ORR mechanism can be outlined below through these sequential steps:

    2(*)+O2→*O+*O

    (1)

    2*O+2H++2e−→2*OH

    (2)

    2*OH+2H++2e−→2H2O

    (3)

    The overall reaction is O2 + 4H+ + 4e− → 2H2O (1.229 V vs. SHE, pH 0).

    Figure 2

    Figure 2.  4e− and 2e− processes of ORR with association and dissociation pathway diagram.

    Under alkaline conditions, the ORR follows a dissociative pathway involving these steps.

    2(*)+O2→*O+*O

    (4)

    2(*O)+2H2O+2e−→2(*OH)+2OH−

    (5)

    2(*OH)+2e−→2(*)+2OH−

    (6)

    The overall reaction is O2 + 2H2O + 4e− → 4OH− (0.401 V vs. SHE, pH 14).

    In acidic environments, the associative mechanism progresses through these stages:

    (*)+O2→*O2

    (7)

    *O2+H++e−→*OOH

    (8)

    *OOH+H++e−→*+H2O2(2e−pathway)

    (9)

    *OOH+H++e−→*O+H2O(4e−pathway)

    (10)

    *O+H++e−→*OH(4e−pathway)

    (11)

    *OH+H++e−→(*)+H2O(4e−pathway)

    (12)

    The primary electrochemical processes involve two distinct routes, i.e., O2 + 2H+ + 2e− → H2O2 (2e− pathway, 0.695 V vs. SHE, pH 0) and O2 + 4H+ + 4e− → 2H2O (4e− pathway, 1.229 V vs. SHE, pH 0). Notably, hydrogen peroxide can undergo further reduction under acidic conditions through H2O2 + 2H+ + 2e− → 2H2O (1.776 V vs. SHE, pH 0). The suggested ORR routes through an associative mechanism in alkaline environments follow these sequential steps:

    (*)+O2→*O2

    (13)

    *O2+H2O+e−→*OOH+OH−

    (14)

    *OOH+e−→*O+OH−(4e−pathway)

    (15)

    *O+H2O+e−→*OH+OH−(4e−pathway)

    (16)

    The overall reaction is O2 + 2H2O + 4e− → 4OH− (4e− pathway, 0.401V vs. SHE, pH 14).

    Crystalline lattice strain represents the discrepancy from the equilibrium atomic spacing within a material's structural framework [50]. Strain (ε) is calculated as the change in lattice parameter (astrained) normalized to the unstrained original (aoriginal) (Eq. 17).

    (ε)=(astrained−aoriginalaoriginal)×100%

    (17)

    This formulation can be used to accurately assess the strength of compressive or tensile strain occurring inside or on the surface of the electrocatalysts. The strain of electrocatalytic materials is usually caused by changes in atom-atom bond lengths or lattice mismatches. Surface strain is defined as lattice distortion in the surface atomic layer of a catalyst, which may differ from bulk lattice strain. It primarily arises from changes in the coordination environment of surface atoms, interfacial interactions, or defect distribution. Through the design, adjustment or control surface strain, electrocatalysts may have different electronic structures and active sites, optimizing the adsorption capacity for reactants, reaction intermediates and products [51-57].

    Under the lattice strain, the crystal structure parameters shrink or stretch accordingly, and the decrease or increase of the spacing among atoms leads to the increase or decrease of the orbital overlapping, changing the filling state of the d-band, which is mainly reflected in the downshift or upshift of the d-band center. According to the d-band center theory proposed by Nørskov [51], there is a linear relationship between strain and d-band center (εd), that is, tensile strain can increase the εd of the post-transition metal (d electron number ≥ 5) and enhance the metal adsorption interaction (Figs. 3a and b), while compressive strain shows in an opposite manner. When subjected to lattice strain, the structural parameters of crystals undergo contraction or expansion, with corresponding alterations in interatomic distances. This dimensional variation modifies orbital overlap characteristics, consequently affecting d-band electron occupancy levels as manifested through downward or upward shifts in the d-band center position (εd). Nørskov's d-band center theory [51] establishes a linear correlation between applied strain and εd values. Specifically, tensile strain elevates the εd in post-transition metals (with d-electron counts ≥5), thereby strengthening metal-adsorbate interactions (Figs. 3a and b), while compressive strain exhibits contrasting effects on these electronic properties.

    Figure 3

    Figure 3.  Correlation between strain effects and d-band center characteristics. (a, b) Schematic representations demonstrating tensile strain's impact on d-orbital alignment in early/late transition metal systems. Reproduced with permission [50]. Copyright 2017, Springer Nature. (c) Visualization depicting Pt-Pt interatomic spacing and interfacial geometry in Pt-skin/intermetallic core structures. (d) Comparative analysis of calculated versus measured overpotentials for various intermetallic compositions relative to Pt's d-band center position. Reproduced with permission [52]. Copyright 2023, Wiley-VCH. (e) Thermodynamic potential profile diagram. (f) Computational modeling of overpotential variations with applied tensile strain on ordered PtNi surfaces Reproduced with permission [54]. Copyright 2020, American Chemical Society.

    Therefore, the introduction of compressive strain can weaken the adsorption of oxygen species and improve the catalytic activity for catalysts with strong oxygen species adsorption. For example, Cheng et al. [52] constructed Pt-skin with controllable thickness on the surface of the prepared chemically ordered intermetallic PtCo nanoparticles (L12-PtCo@ML-Pt/NPCs) (The structure of L12 intermetallic compounds is similar to diamond crystals). The lattice compressive strain of Pt-skin can be precisely controlled by adjusting the composition of the Pt-core and the thickness of Pt-skin (Fig. 3c), so as to effectively reduce the excessive adsorption of Pt sites to ORR reaction intermediates and improve ORR performance. It is found that compared with materials alloying with other metals (Cr, Mn, Fe, Zn), L12-Pt3Co @ML-Pt/NPC exhibits the most suitable compressive strain and the catalytic performance is closest to the “volcano” peak of catalytic performance (Fig. 3d). On the contrary, Yang et al. [54] reported on the tensile strain introduced by the formation of an intermetallic phase and N-doping case denoted as PtNiN. As shown in Fig. 3e, the DFT results indicated that strong adsorption of *OH makes the formation of the second H2O molecular being the potential-determining step (PDS) and the optimum tensile strength (0.2%-1.5%, Fig. 3f) is able to weaken the adsorption of all intermediates, especially for *OH, reducing the energy barriers for the formation of H2O. This study was the pioneering work that reported the tensile strain regulation in PtNiN alloys, providing both theoretical and experimental evidences for the application of tensile strain to optimize the ORR performance.

    Evidently, applied strain modifies the electronic configuration through alterations in interatomic spacing at surface layers, consequently enhancing catalytic efficiency, a critical factor for developing and optimizing high-performance ORR catalysts. During heterogeneous catalyst fabrication, structural features including alloy compositions [55], core-shell structure [56], size and morphology, defects in substrates [57], will introduce lattice mismatch or atomic bond length changes, resulting in strains (Fig. 4). In the following, five strategies to manifesting strain and the mechanism of regulating ORR performance will be addressed in detail.

    Figure 4

    Figure 4.  Strategies to induce strain. (a) Schematics of strain-enhanced Pt-Co bimetallic solid solutions. Reproduced with permission [55]. Copyright 2024, Springer. (b) Illustration of lattice mismatched epitaxy introduced compressive strain in core-shell nanoparticles. Reproduced with permission [56]. Copyright 2019, American Chemical Society. (c) Visual explanations of lattice deformation mechanisms, adsorbate-transition metal interactions, and upward shifts in d-band center positions. Reproduced with permission [58]. Copyright 2024, Wiley-VCH. (d) Surface strain caused by particle size/shape. Reproduced with permission [56]. Copyright 2019, American Chemical Society. (e) Strain formation at crystalline interface boundaries or structural defects (hole). (f) Surface curvature effect caused strain. Reproduced with permission [57]. Copyright 2023, American Chemical Society.
    2.2.1   Strain of alloy structure

    When two or more sorts of metals form a solid solution or one phase, their atomic radii are different which leads to changes in the lattice parameters compared with pure metals. This variation causes local strain, especially in the vicinity of interfacial region. Regarding ORR electrocatalysis, substantial research has focused on platinum alloy systems incorporating transition metals (denoted as PtM, where M represents Mn, Fe, Co, Ni, Cu, etc.), as documented in references [58-66] and illustrated in Fig. 5a. A notable example involves carbon-supported PtMn/C catalysts developed by Yang's team [66], where manganese's reduced atomic dimensions caused measurable lattice contraction. Comparative analysis revealed the PtMn system's (111) and (200) plane spacings decreased to 0.22 and 0.19 nanometers respectively, contrasting with pure platinum's standard values of 0.23 nm (111) and 0.20 nm (200), as visualized in Fig. 5b. These crystallographic deviations produce measurable strain phenomena within catalytic materials, manifested through bond length alterations detectable via X-ray photoelectron spectroscopy analysis. X-ray absorption spectroscopy (XAS) and extended X-ray absorption fine structure (EXAFS) characterizations (Fig. 5c) reveal that the lattice contraction in PtMn alloys modifies the electronic configuration and diminishes bonding interactions between platinum atoms and ORR intermediates, consequently accelerating ORR kinetics. Elevated manganese concentrations induce progressive shortening of Pt-Mn bond distances relative to pure platinum (2.761 Å reference). Wavelet transform analysis (Fig. 5d) quantifies this structural evolution, showing bond lengths of 2.751 Å (Pt79Mn21), 2.749 Å (Pt56Mn44), and 2.740 Å (Pt42Mn58) corresponding to lattice contractions of 0.36%, 0.43%, and 0.76% respectively. The optimized Pt56Mn44/C catalyst demonstrated superior electrochemical performance with a half-wave potential (E1/2) of 0.910 V in acidic media, surpassing both other PtMn variants (35-70 mV enhancement) and commercial Pt/C benchmarks. This performance hierarchy underscores the critical role of controlled lattice strain in catalytic enhancement. Comparative Tafel analysis further confirmed enhanced charge transfer kinetics for the Pt56Mn44/C catalyst, as evidenced by reduced slope values relative to conventional platinum catalysts. The correlation between MA/SA and compressive strain displays a complex non-linear pattern. Experimental data reveals Pt56Mn44/C catalyst demonstrates enhanced electrochemical performance with mass activity reaching 0.53 A/mgPt and specific activity attaining 1.0 mA/cm2. These values represent significant improvements, surpassing those observed in commercial Pt/C by factors of 4.4 and 5.0 respectively when comparing equivalent strain conditions (Figs. 5e and f).

    Figure 5

    Figure 5.  Strain in alloys. (a) Schematic illustration of strain effect in PtM alloy. Reproduced with permission [59]. Copyright 2023, American Chemical Society. (b) HAADF-STEM images of Pt56Mn44 nano-dendrites. (c) XPS spectra of Pt 4f orbitals alongside EXAFS evaluations at the Pt L3 absorption edge and (d) multiscale wavelet transformation patterns. (e) Comparative Tafel slope analysis, (f) ORR catalytic metrics including SA and MA (0.9 V vs. RHE) across various electrocatalysts. Reproduced with permission [66]. Copyright 2024, Wiley-VCH. (g) Activity-structure correlations mapping mass performance against Pt-Pt bond distances in PtMnM/C versus PtMn/C systems. (h) Electronic parameter relationships connecting catalytic activity with d-band center positions. (i) Mechanistic illustration of strain/electronic configuration impacts on intermediate adsorption in PtMnM alloys. (j) Performance benchmarking of PtMnCo/C against conventional catalysts through MA/SA measurements. Reproduced with permission [68]. Copyright 2024, Science China Press. (k) AC-STEM images and the corresponding GPA images for axial strain (εxx) and shear strain (εxy). (l) Bader charge analysis and (m) the d-band center of different elements in HEANs. (n) ORR polarization of Tafel plots, and onset potential at 1600 rpm for HEAN/CNT and Pt/C. Reproduced with permission [71]. Copyright 2024, the Author(s).

    Recent studies have demonstrated significant advancements in atomic arrangement engineering of alloy components, leading to the development of novel class of ordered materials termed intermetallic compounds. These structurally defined materials have attracted considerable attention in electrocatalytic applications [67,68]. Wang et al. [68] reported the carbon-supported PtMn-M ternary intermetallic compound catalyst (PtMn-M/C, Fig. 5i), whereby Mn element in the binary intermetallic compound PtMn was replaced by a third transition metal, and the surface strain is induced. Changing the sorts of transition metal elements can regulate the indicated strain and optimize the Pt-Pt atomic spacing and the d-band center of Pt, thus effectively weakening the strong adsorption of Pt site to the reaction intermediate. Electrochemical testing showed that the ORR activity of PtMn-M/C showed a volcanic relationship with the PtMn-Co/C atomic spacing and d-band center, respectively (Figs. 5g and h). The PtMn-Co/C with the optimal strain showed excellent activity and durability, i.e., the MA at 0.9 V vs. RHE was 1.06 A/mgPt, 4.6 times that of commercial Pt/C. In addition, the E1/2 decreased by only 10 mV after 50k accelerated deterioration test (ADT) cycles, much better than commercial Pt/C catalysts (Fig. 5j).

    High-entropy alloys (HEAs) [69] are composed of a variety of elements mixed in equal proportions or approximately equal proportions, without single alloying element dominating, which breaks the design concept of traditional alloys. HEA exhibit excellent properties in mechanical properties, corrosion resistance, thermal stability, etc., which also show promising prospects in electrocatalytic field. The inherent atomic size variations among constituent elements induce substantial lattice strain, enabling precise modulation of electronic configurations and catalytic efficiency [70,71]. In a notable study, He et al. [71] synthesized Pt-Fe-Co-Ni-Cu HEA nanoparticles and employed geometrical phase analysis (GPA) for strain characterization. Their findings revealed concurrent axial (εxx) and shear (εxy) strain distributions peaking at 5% magnitude (Fig. 5k), directly correlating with observed lattice distortion patterns. GPA tests in this study were performed using a JEOL JEM-ARM200F aberration-corrected transmission electron microscope at an acceleration voltage of 200 kV, with a scanning step size of 0.2 nm. The strain effect in HEANs can regulate the adjacent atoms to re-distribute the local charge, which increases the charge transfer and spin polarization between Pt and other elements. As shown in Fig. 5l which is the Bader charge analysis, charge transfer occurs among different elements, for instance, charge accumulation on Pt is observed, ranging from 0.37 |e| to 0.69 |e|, while other transition metal elements are positively charged, resulting in optimal adsorption potential which reduces the overpotential of the catalytic reaction. It is seen that finite spin polarization is induced for Fe, Co and Ni sites (Fig. 5m), which is conducive to the adsorption of O2. Moreover, the wide distribution of d-band centers in HEANs endows it good possibility to provide different active sites for various intermediates during different reactions. Fig. 5n compares the changes of the onset potential (Eonset) and the Tafel slope before and after the cycle of the commercial 20% Pt/C catalyst, whereby those of the HEANs performs better and remains without significant difference after the recycling. Moreover, there is negative change in the initial potential.

    In some alloy systems, a transition from one crystal structure to another may occur as the temperature changes, which introduces strain [72,73]. Liang et al. [73] used Co doping to regulate the crystal phase transition of PtCu alloy and studied the phase evolution of PtCoxCu1-x alloy with different Co contents and its effect on the activity of ORR. The results showed that with the increase of Co content, the formation energy of the L10 phase decreases, that is, when 20% of Cu is replaced by Co, the PtCu0.8Co0.2 catalyst forms in the L10 phase, which showed a larger compressive strain (-6.9%) compared with that of L11-PtCu catalyst (-3.8%). As a result, the ORR intermediates bind more weaker on the L10-PtCu0.8Co0.2 surface, along with a downshift of the d-band center. In a H2-O2 single-cell test, the L10-PtCu0.8Co0.2 catalyst exhibited a MA of 0.95 A/mgPt at 0.9 V vs. SHE, which is superior to those of Pt/C (0.43 A/mgPt) and L11-PtCu (0.87 A/mgPt).

    As discussed, the relationship between strain and ORR catalytic performance in the alloy catalyst is complex and subtle, which plays a critical role in deciding its electronic structure, geometry and phase stability. Alloying, by optimizing the composition ratio of precious metal-based materials, can significantly reduce the loading of precious metal elements while maintaining or enhancing their catalytic performance, which is a promising modification strategy for noble metal catalysts.

    2.2.2   Strain of core-shell structure

    The core-shell configuration facilitates accurate adjustment of interfacial strain through lattice parameter discrepancies between constituent layers, representing a widely adopted approach for controlled strain engineering. This interfacial strain originates primarily from variations in lattice constants between core and shell components, inducing structural deformation at their contact interface [74-76]. The main ingredients affecting the strain of core-shell structure are manifested in the following two aspects.

    Firstly, the arrangement of atoms at the interface is forced to adjusting the lattice difference [77-80]. The composition and morphology of core-shell catalysts can be precisely controlled by electrochemical methods, colloid synthesis and chemical reduction methods. Zhang et al. [77] prepared a core-shell catalyst with L10 intermetallic compound FePt as the core and PtBi alloy as the shell. The interlayer compression caused by the high content of small-size transition metal Fe in the FePt core and the in-plane shear caused by a small amount of large-size Bi in the PtBi shell imposes a strain in the catalyst surface, enhancing the contraction of the Pt-Pt bond in the vicinity of the catalyst surface. EXAFS analysis and wavelet analysis (Figs. 6a and b) revealed significantly shortened Pt-Pt bond lengths in FePt@PtBi (2.36 Å) and FePt (2.40 Å) compared to Pt/C (2.77 Å), primarily due to Fe's lattice contraction effect. Further analysis demonstrated Bi's crucial function in modulating surface electronic states through strain engineering. The formation of additional compressed Pt-Pt bonds was quantitatively demonstrated. Fig. 6c reveals substantial lattice contraction (averaged -4.6%) occurring at FePt@PtBi nanoparticle surfaces, with comparatively milder compression observed in pure Pt (-1.1%) and FePt (-2.6%) systems. Experimental calculations indicated Pt (111) surfaces subjected to compressive strain exhibited lower oxygen adsorption energies by 0.39 eV compared to strain-free counterparts, confirming weakened molecular adsorption. Previous studies [80] have established that such compressive lattice distortions reduce adsorbate binding energies on densely packed crystalline planes, thereby improving ORR efficiency. The FePt @PtBi catalyst shows excellent electrocatalytic ORR activity and stability, i.e., the MA was 0.96 A/mgPt, and the MA remains at 0.79 A/mgPt even after 30,000 cyclic voltammetry ADTs. Gao et al. [79] reported a carbon-supported intermetallic core-shell nanoparticle catalyst (fct-PtCo @PtIr/C) (Fig. 6d). The core is composed of face-centered tetragonal (fct) intermetallic nanocrystals whereby Pt and Co atoms stack ordered (L10 structure), and the interface with Pt-Ir layer can generate 1%-3% compressive strain, as shown in the GPA (Fig. 6e). The Pt-Ir shell with compressive strain shortens the length of the Pt-Pt bond between the surface Pt atoms, thereby downshifting the d-band center of platinum atoms and weakening oxygen-containing intermediates' adsorption strength, crucial factors for enhanced ORR kinetics. Electrochemical evaluations revealed the fct-PtCo@PtIr/C composite catalyst demonstrates superior MA (1.17 A/mgPt+Ir) and SA (2.63 mA/cm2Pt+Ir) (Fig. 6f), which are 5.85 and 8.48 times higher than those of Pt/C (0.2 A/mgPt and 0.31 mA/cm2Pt), respectively.

    Figure 6

    Figure 6.  Strain in core-shell catalysts. (a) Fourier-transformed k3-weighted Pt L-edge XANES spectra and (b) wavelet analysis patterns for FePt@PtBi systems, compared to FePt and Pt/C reference materials. (c) Chromatic mapping illustrating lattice distortion patterns across Pt, FePt, and FePt@PtBi structures Reproduced with permission [77]. Copyright 2021, Wiley-VCH. (d) Structural model demonstrating strain distribution in fct-PtCo@PtIr/C heterostructures. (e) GPA strain image. (f) Catalytic performance metrics showing mass-normalized and surface-specific activities at 0.9 V vs. RHE Reproduced with permission [79]. Copyright 2023, Wiley-VCH. (g) Synthetic process of Se2-Pt NPs and corresponding structural evolution on the surface. Surface structures of Se1-Pt NPs and Se3-Pt NPs. (h) The d-band centers of the active-site Pt atoms in various catalysts. (i) The 2e−/4e− ORR path and corresponding energy barriers for Se2-Pt and Se3-Pt. (j) Values of the selectivity (%). Reproduced with permission [81]. Copyright 2024, Nature. (k) Atomic-resolution HAADF-STEM and (l) HRTEM micrographs of mesoporous Pt@Pt-skin Pt3Ni core-shell frameworks. (m) Diffraction intensity comparisons between bulk Pt (111) planes and Pt-skin surfaces revealing ~4.9% compressive lattice strain. MA and SA variations observed in the mesoporous Pt@Pt-skin Pt3Ni CSFWs/C electrocatalyst. Reproduced with permission [82]. Copyright 2023, Nature.

    Secondly, the thickness of the shell directly affects the strength and distribution of strain [81,82]. Experimental observations reveal that expanding the amorphous coating dimensions amplifies interfacial deformation effects. In their investigation, Yang's team [81] engineered a core-shell catalytic system with tunable Pt-Se amorphous layer dimensions, where distinct lattice mismatch-induced stress patterns became evident through structural analysis (Fig. 6g). Precise control over the amorphous coating's dimensional parameters was achieved through controlled selenization levels (Sex-Pt NPs, where x indicates selenization intensity). Computational simulations (Figs. 6h and i) demonstrated that optimal coating dimensions (Se2-Pt configuration) induce downward shifting of the Pt site's d-band center, effectively reducing *OOH adsorption intensity while promoting selective H2O2 generation through the 2e− pathway, achieving remarkable selectivity exceeding 95% (Fig. 6j). Comparative analysis of reaction pathways revealed substantially lower activation barriers for the 2e− process versus the 4e− alternative in both catalytic systems, confirming the dominance of the former mechanism (Fig. 6i). Liu et al. [82] developed anisotropic mesoporous Pt@Pt-skin Pt3Ni core-shell framework nanowires (CSFWs), with structural details revealed through HAADF-STEM imaging. These images demonstrate a sub-5nm platinum nanowire core integrated with a three-dimensional interconnected mesoporous network (2-5 nm pores) within a nanostructured gourd-shaped Pt3Ni framework shell (Figs. 6k and l). The Pt-skin layer measured approximately 1-1.5 nm in thickness, equivalent to 5-8 atomic layers, demonstrating enhanced platinum utilization efficiency for catalytic applications. Crystallographic analysis revealed a 2.16 Å interatomic spacing in the Pt lattice, representing 4.9% contraction compared to standard Pt (111) planes (2.27 Å spacing) (Fig. 6m). This curved hollow framework architecture not only maximizes electrochemical active surfaces but also induces compressive lattice strain that optimizes surface electronic properties. In ORR test, the anisotropic mesoporous Pt@Pt-skin Pt3Ni core-shell frame nanowires showed excellent MA and SA (Fig. 6n), which were 6.69 A/mgPt and 8.42 mA/cm2 at 0.9 V, respectively. The catalyst also showed high stability, i.e., the E1/2 of the mesoporous Pt@Pt-skin Pt3Ni CSFWs shifts negatively of only 4 mV after 50,000 cycles. The SA and MA of mesoporous Pt@Pt-skin Pt3Ni CSFWs were reduced by only 2.9% and 2.8% after 50,000 cycles, respectively.

    2.2.3   Strain caused by the size and shape change

    Nano-catalysts have become the mainstream of research because of their high atomic utilization and catalytic efficiency. The size and shape change of the catalyst demonstrate important impact on the catalytic activity in ORR [83,84]. Nanoparticles with smaller size generally bear with large lattice compressive strain due to the fact that the higher specific surface area of the small nanoparticles brings more surface atoms which has to be compressed to reduce the chemical potential [85,86]. Moreover, crystallographic facets and geometric configurations further modulate strain distribution patterns, with deliberate manipulation of these parameters proving effective for catalytic enhancement. Concurrently, induced lattice strain contributes to minimizing thermodynamic instability in nanocrystalline materials, thereby preserving active site integrity and prolonging operational lifespan under reaction conditions [87-93].

    Xia et al. [87] developed a bimetallic octahedral nanocrystalline structure (Fig. 7a) featuring a fct-PtCo intermetallic core enveloped by a three-to-four atomic layer platinum shell oriented along the (111) crystallographic plane, with uniform particle dimensions measuring 8 nm. The X-ray diffraction pattern (Fig. 7b) reveals characteristic peaks corresponding to the face-centered cubic structure of platinum (JCPDS No. 04-0802), though with discernible peak shifts indicating partial substitution of larger Pt atoms (1.39 Å) by smaller Co atoms (1.26 Å), resulting in lattice contraction. Thermal annealing at 600 ℃ for 4 h induced structural ordering, evidenced by emerging diffraction peaks at 24° and 33° 2θ values corresponding to fct-PtCo (JCPDS No. 65-8969) (001) and (110) planes respectively. The observed high-angle shift of the (111) diffraction peak suggests enhanced Pt-Co alloying during thermal processing. Subsequent conformal platinum deposition maintained all structural features without altering peak positions or full-width at half-maximum values, confirming structural preservation during surface modification. The (111) slight downward shift of the diffraction peak indicates that the Pt content in the nanocrystals increases slightly. Structural incompatibility between fct-PtCo and fcc-Pt phases generates asymmetrical peak profiles in fct-PtCo@Pt nanocrystals, indicative of substantial interfacial lattice strain at phase boundaries. At the same time, the anisotropic surface strain also helps to reduce the surface energy of the nanocrystals, thus stabilizing the active Pt surface and preventing dissolution during the catalytic process. Fig. 7c showed changes in MA for different catalysts before and after ADTs, the MA of Pt/C, fcc-PtCo/C and fct-PtCo/C catalysts decreased by 57%, 60% and 35% after 10,000, 20,000 and 30,000 cycles respectively, confirming the potential of fct-PtCo@Pt as an ORR catalyst.

    Figure 7

    Figure 7.  Strain effects based on size/shape characteristics. (a) Structural diagrams of fcc-PtCo, fct-PtCo/C, and fct-PtCo@Pt/C catalysts, along with their corresponding (b) XRD diffraction profiles. (c) Catalytic performance metrics showing MA comparisons. Reproduced with permission [87]. Copyright 2021, American Chemical Society. (d) Average particle size (indicated by black lines) and (e) MA and SA measurements for PtMo/C-X catalysts synthesized at varying temperatures (200-1000 ℃). Reproduced with permission [92]. Copyright 2022, American Chemical Society. (f) Architectural visualization of the CS-Pt/C catalyst system. (g) Computed surface strain patterns and *OH adsorption energy simulations on Pt cone. (h) LSV profiles during accelerated durability testing cycles, comparing the MA and SA of CS-Pt/C catalysts pre- and post-stability evaluations. Reproduced with permission [93]. Copyright 2024, Wiley-VCH. Mechanistic representations of 2e− ORR toward hydrogen peroxide generation using (i) S- and (j) L-ZnO nanoplate catalysts. AFM topographic mappings with elevation analyses for (k) S- and (l) L-ZnO nanoplates along designated transects. (m) Comparative Gibbs free energy variations and (n) electronic density of states (DOS) characteristics for S- versus L-ZnO configurations during 2e− ORR processes. Reproduced with permission [94]. Copyright 2023, Royal Society of Chemistry.

    Reduced dimensions in electrocatalysts generally enhance geometric surface exposure, a critical parameter for optimizing ORR efficiency [90-93]. This size-dependent phenomenon presents a paradox, as sub-5 nm particles demonstrate increased structural defects that inversely affect SA. While balancing SA with electrochemical surface area (ECSA) remains challenging, precise particle size regulation emerges as a crucial strategy for maximizing catalytic performance. Kim's team [92] engineered carbon-supported PtMo alloys through gas-phase synthesis, achieving optimal 3.1 nm particles through 800 ℃ annealing (PtMo/C-800). This thermally processed catalyst demonstrated a remarkable MA of 46 mA/mgPt and maintained exceptional stability during ADTs (Figs. 7d and e). Liu et al. [93] reveloped innovative conical platinum nanostructures (CS-Pt/C) with compressed (111) facet configurations while maintaining ultra-small 2 nm dimensions (Fig. 7f). As shown in Fig. 7g, the slight tensile strain observed at the inner edges, most outer and inner surface atoms experience a compressive strain of 0.5% to 2.5% relative to the bulk Pt. The high SA of CS-Pt/C could be attributed to an interplay between the coordination number and strain distribution of the surface atoms. Pt cones are predominantly covered by (111) facets in both the exterior and interior surface of the cones and the compressively-strain on (111) facets enhance the intrinsic SA of Pt (111) toward ORR by weakening the interaction between the surface and OH. Since the high SA of CS-Pt/C (0.99 mA/cm2), it is not surprising to see that the MA of CS-Pt/C catalyst (1.72 A/mgPt) is 6.4 times higher than that of Pt/C. Even after 20 000 potential scanning cycles in 0.6-1.1 V vs. RHE, the CS-Pt/C catalyst still showed 5.3 times higher MA than the initial value of Pt/C. And the E1/2 decreased by 1.3 mV for the CS-Pt/C catalyst. Meanwhile, there was almost no change to the SA of CS-Pt/C (Fig. 7h).

    On the contrary, Chen et al. [94] proposed a concept of inverse size effect to facilitate the efficient generation of H2O2 at ampere-level current density. Specifically, the authors studied ZnO catalysts of different size and found that the catalytic activity increased significantly with increasing size. Structural analyses confirmed the distinct sizes of S-ZnO (1.7 nm) and L-ZnO (87.7 nm) through electron microscopy observations (Figs. 7k and l). Crucially, the *OOH intermediate exhibited divergent adsorption behaviors with binding energies of 0.6983 eV on S-ZnO versus -0.5084 eV on L-ZnO (Fig. 7m), suggesting thermodynamically favorable stabilization of this critical reaction intermediate on the larger catalyst. This observation aligns with charge redistribution patterns visualized in differential density plots (Figs. 7i and j), where intensified electron-proton exchange occurs at L-ZnO/*OOH interfaces. Additional evidence emerges from electronic structure analysis, where the pronounced density of states peak near the Fermi level in L-ZnO corroborates strengthened *OOH surface interactions (Fig. 7n). As a result, the L-ZnO nano-disk performs ~100% H2O2 selectivity at ampere-level current density ( > 1 A/cm2).

    2.2.4   Strain caused by defects

    Deficiency is ubiquitous in materials, which causes inhomogeneous strain fields and can be utilized in improving the activity of ORR for targeted catalysts. Intrinsic defects such as vacancies, gap atoms and steps are the origin of local lattice distortions [95-98], which affects the structural geometry and electronic structure of the catalyst, changing the adsorption energy of reactants on the catalyst surface and optimizing the catalytic activity of ORR [48,99-101].

    Zeng et al. [48] revealed that nanoscale imperfections like atomic steps can disrupt surface symmetry, causing surface stress dissipation, rearrangement of surface atoms, and formation of multi-nanometer scale heterogeneous strain fields. Their study illustrates the inherent tensile stress present in Pt (hhl) terraces along with the spontaneous stress relief mechanism achieved through symmetry disruption and compressive strain generation as demonstrated in Fig. 8a. They compared the side view of the Pt (hhl) step surface at different terrace widths (1-10 nm) with the atomic site resolution of the surface strain (Figs. 8b and c). The results show that the stress release and surface strain are inversely proportional to terrace step width, that is, with the increase of the terrace step width, the stress release and strain of the surface decrease. Indeed, both the d-band center, the *OH adsorption energy and the surface strain are sensitive to the geometric location of the atomic site and the terrace width (Figs. 8d and e). Analysis of d-band orbital positions reveals systematic negative displacements across surface atoms, correlating directly with compressive stress magnitudes. In Pt (21 21 20) systems, edge-proximal platinum atoms experiencing -3.7% lattice distortion demonstrate 0.1 eV downward displacement, contrasting with minimal 0.01 eV shifts observed at terrace centers (-0.3% strain). This displacement phenomenon exhibits terrace-width dependency, with extreme values reaching 0.14 and 0.08 eV respectively. Spatial stress analysis reveals non-uniform compressive stress distribution across stepped surfaces, characterized by intensified deformation near step peripheries compared to terrace midpoints. Notably, compressive relaxation occurs at central step positions as terrace dimensions expand. The synergistic effect of severe lattice compression (-3.7%) and attenuated *OH binding near step edges creates localized high-activity zones, forming catalytic hot spots through atomic-scale strain engineering. Catalytic performance exhibits an exponential dependence on the binding energies of reaction intermediates. Mesa atoms located two atomic columns above and below the edge of the step were found to be the sites with the highest ORR activity, with up to 50 times the ORR improvement factor (Fig. 8e). This study was the first to confirm that defects (e.g., atomic steps) on Pt (111) stepped surfaces break surface symmetry, release surface stress, and generate inhomogeneous strain fields spanning multiple nanometers.

    Figure 8

    Figure 8.  Strain by defects. (a) The relationship between surface stress release and surface strain generation of stepped Pt (111) surfaces. (b) Side view (upper panels) and atomic site-resolved surface strain (lower panels) of Pt (332), and (c) Pt (21 21 20) surfaces with terrace width from 1.3 nm (n = 5) to 10.1 nm (n = 41), as indicated by double arrow lines. Surface sites correspond to atoms in the top layer of the side views. (d) Side view (upper panels) and atomic site-resolved d-band center shift (dεd), (e) OH adsorption energy shift and predicted ORR improvement factors of Pt (21 21 20) surfaces with respect to that of the Pt (111) surface. Reproduced with permission [48]. Copyright 2024, Nature. (f) Diagram of the relationship between atomic arrangement and (g) coordinative shell, atomic PDFs of Vac-NiPt, NPs/NG, Vac-Pt NPs/NG and commercial Pt/C. (h) Histogram about kinetic current density, SA and MA of Vac-NiPt NPs/NG, Vac-Pt NPs/NG, and Pt/C at 1600 rpm and -0.85 V vs. RHE. (i) Negatively polarized LSV curves of Vac-NiPt NPs/NG and Pt/C before and after 50 k, 100 k and 200 k cycles Reproduced with permission [101]. Copyright 2025, Wiley-VCH.

    Yan et al. [101] synthesized PtNi/C catalyst by zeolitic imidazolate framework-8 (ZIF-8) pyrolysis method, and introduced atomic-scale vacancy defects on Pt nanoparticles by vaporization of Zn (Vac-NiPt NPs/NG). In addition to the EXAFS which is merely sensitive to the short-range local structure of near-neighbor coordinative shell ( < 3 Å, corresponding to 1st and 2nd shells shown in Fig. 8f), the atomic pair distribution function (PDF) was also used to further investigate the long-range local structure of Pt NPs. As shown in Fig. 8g, the atomic PDFs G(r) pattern clearly exhibits 10 Pt-Pt coordinative shells within the 2-11 Å range. The observed deviation of peaks in Vac-NiPt NPs/NG and Vac-Pt NPs, when compared to Pt/C, serves as an evidence for lattice distortions. Vac-NiPt NPs/NG exhibit a shorter distance of the closest Pt-Pt path, this result is in accordance to that of EXAFS, the average distances of the 2nd, 4th, 6th, 9th, and 10th Pt-Pt coordinative shells in Vac-NiPt NPs/NG were observed to be shorter when compared to Pt/C, while the average distances of the 3rd, 5th, 7th, and 8th Pt-Pt coordinative shells were tensile. These findings demonstrate that a large number of atomic-scale vacancy defects contribute to long-range tensile and compressive strains in Pt NPs. As summarized in Fig. 8h, Vac-NiPt NPs/NG displayed high kinetic current density of 15.03 mA/cm2, specific activity (SA) of 2.27 mA/cm2 ECSA and MA of 1683 A/gPt, surpassing those of Pt/C by 1.65, 15.90 and 9.43 times, respectively, suggesting that Vac-NiPt NPs/NG presented great ORR activity and Pt utilization. Furthermore, ADT performed by continuous repetitive CV cycling was carried out to evaluate the durability. As depicted in Fig. 8i, Vac-NiPt NPs/NG merely exhibited slight catalytic activity attenuation after 200000 cycles.

    2.2.5   Strain caused by the substrate

    Interactions between the substrate and active components impose external constraint strain. This strain regulation method is particularly suitable for synergistically optimizing the stability and activity of single-atom and cluster catalysts. Single atoms and clusters require substrates to maintain their structure and stability, which are prone to agglomeration, migration, or decomposition due to high system energy. The selection of substrates is usually based on their compatibility and stability to the target system [102,103]. For example, for single atom catalysts, carbon materials substrates are favorable because their excellent mechanical property provide satisfying space and chemical environment to stabilize individual atoms without affecting their catalytic activity [104,105].

    The properties of the substrate, including surface structure, chemical composition, and electronic properties, can significantly affect the performance of the catalyst. In general, the morphological features of the substrate, such as edges, steps, and sharp corners, are able to concentrate stress, causing metal atoms nearby in a highly distorted state [106,107]. Nano-scale substrates are more likely to develop strong strain effects at the interface due to their high curvature [108-110]. Liu et al. [109] loaded Co single atom onto a highly arcuated carbon layer (Co-SAC) with a very small radius of curvature (about 2 nm) to generate compressive strain. The local compressive strain induced the redistribution of electrons in different spatial orientations of d orbitals of Co atom, and increased the number of electrons filled in the radial (xy plane), thus enhancing the effective overlap of electron orbitals with active intermediate molecules and improving the ORR activity. Feng et al. [110] reported a Fe-N-C catalyst with dense FeN4 sites on stratified porous carbon with high curved surfaces (Fe-N-hcC), (Fig. 9a) and the curvature (c, c = 1/R, R refers to the radius of the sphere) of the onion-like carbon was calculated to be ≈0.023 (Fe-N-C-0.023). The Fourier transform EXAFS spectrum (Fig. 9b) showed that Fe-N-C and Fe-N-hcC are approximately 1.50 Å and are attributed to the first coordination shell scattering of the Fe-N bond. The mean Fe-N bond spacing in Fe-N-hcC is longer than that in Fe-N-C, which is mainly due to the local strain effect of bent onion-like carbon in Fe-N-hcC. The d-band center of Fe-N-C-0.023 is -1.871, which is lower than the -1.831 of Fe-N-C, which weakens the adsorption capacity of *OH intermediates (Fig. 9c), thus accelerating the overall ORR kinetics. At 0.85 V, the dynamic current density (Jk) of Fe-N-hcC reached 3.87 mA/cm2, and the intrinsic turnover frequency (TOF) of FeN4-hcC reaches 2.22 s−1 at 0.85 V, about 4.2 times that of Fe-N-C (Fig. 9d).

    Figure 9

    Figure 9.  Strain by substrate. (a) High-resolution TEM of Fe-N-hcC. (b) Fourier transformed Fe K-edge EXAFS spectra for Fe-N-C, Fe-N-hcC, and related reference compounds. (c) Correlations between the d-band center for the single Fe sites in FeN4 and the ΔGOH*. (d) Mass activities and TOF values at 0.85 V for the Fe-N-hcC and Fe-N-C electrocatalysts. Reproduced with permission [110]. Copyright 2023, Wiley-VCH. (e) Schematic of the Co-WC structure with both Co superstructure formation. (f) Bonding status and adsorption behavior under pristine (blue) and compressive (red) stress. (g) The stress-induced changes in Co-C bond length. (h) Theoretical overpotential of the catalyst for OER and ORR under different stresses. (i) Bifunctional LSV curves of Co/WC and Pt/C+IrO2 in an O2-saturated 0.1 mol/L KOH solution. Reproduced with permission [111]. Copyright 2024, American Chemical Society.

    In addition, strong interactions at the metal-support interface, such as chemical bonding or physical adsorption between metal and support, can also cause local strains [111-114]. For example, the tight binding of metal atoms to defect sites on the support may make the region around these atoms subject to large tensile or compressive strains. Li et al. [111] proposed to use tungsten carbide as a substrate to synthesize a catalyst (Co-WC) with both superlattice and well-dispersed single atoms. The presence of a Co superstructure induces compressive strain within the structure of WC (Fig. 9e) due to the lattice mismatch between WC and Co, which leads to the shortening of the Co-C bond length (Fig. 9g), thus reducing the d-band center of the transition metal to a low energy region (Fig. 9f), which is conducive to the desorption of intermediates and the acceleration of kinetics. The calculated overpotential for the oxygen evolution reaction (OER) and ORR under different applied lattice strains is illustrated in Fig. 9h. It can be observed that the compressed strain originated from the Co superstructure lowers the overpotential of the OER and ORR to 0.48 and 0.45 V, which significantly accelerates the bifunctional reaction kinetics and thus promote the electrochemical performances of zinc-air battery (ZAB). As shown in Fig. 9i, the prepared Co-WC electrocatalyst exhibited excellent difunctional catalytic activity, i.e., E1/2 = 0.893 V for ORR and Ej=10 = 259 mV for OER, with ΔE = 0.623 V, superior to those of the commercial benchmark Pt/C+IrO2. Impressively, the assembled rechargeable ZAB exhibited an open circuit voltage of 1.48 V and long-term cycle stability of 6000 cycles.

    Ye et al. [112] found that the monodisperse cobalt phthalocyanine (CoPc) supported by single-walled carbon nanotubes (SWCNTs) catalyst (CoPc/SWCNTs) showed improved catalytic performance as a result of the molecular curvature induced by the CNTs (Fig. 10a). The FT-EXAFS spectrum shows the distance between Co-N1 (the first coordination sphere) and Co-C1 (the second coordination sphere) increases as the diameter of the carbon nanotubes decreases (Fig. 10b), which indicates that the CoPc molecule is distorted. The CoPc/SWCNTs demonstrate superior CO2 reduction performance, i.e., it achieves a methanol partial current density of > 90 mA/cm2 and a selectivity of > 60% over 16.6% for multi-walled CNTs. The authors also extended this concept to other catalytic reactions. They investigated the ORR activity of FePc/SWCNTs with different CNT diameter as substrates. The E1/2 of FePc/SWCNTs in ORR was 0.93 V, which was 40 mV higher than that of Pt/C. The electron transfer number of FePc/SWCNTs was 3.98, which was close to the theoretical limit for the four-electron reduction process (Fig. 10c).

    Figure 10

    Figure 10.  Strain analysis of substrate curvature. (a) Depiction of structural deformations in CoPc when deposited on CNTs with varying diameters. (b) EXAFS Fourier analysis comparing CoPc/SWCNTs with CoPc/15, CoPc/50 and pristine CoPc. (c) Comparative analysis of E1/2 values and mean electron transfer counts for FePc/SWCNT, FePc/15, FePc/50 versus commercial Pt/C in oxygenated 0.1 mol/L KOH solution. Reproduced with permission [112]. Copyright 2023, Nature. (d) Thermodynamic free energy comparison between planar and curved FePc-C24 configurations under 0.0, +0.8, and +1.0 V potentials at 298 K. (e) ORR LSV profiles demonstrating durability after 5000 CV cycles for FePc/SWCNT versus 20% Pt/C. Reproduced with permission [113]. Copyright 2025, American Chemical Society. (f) E1/2 performance comparison. (g) Electrochemical stability evaluation of HCNT, Co-N-C@CNT, Co-N-C@HCNT and Pt/C at 1600 rpm in alkaline oxygen environment. (h) Power output characteristics and discharge profiles comparing Co-N-C@HCNT with Pt/RuO2 composite. Reproduced with permission [114]. Copyright 2024, Wiley-VCH.

    Research revealed that molecular strain enhances the reductive desorption mechanism through a 60 meV reduction in the *OH desorption energy barrier (Fig. 10d). ADT demonstrated FePc/SWCNT's exceptional stability, as evidenced in Fig. 10e. Following 5000 cyclic voltammetry scans between 0.6-1.0 V, FePc/SWCNT exhibited minimal E1/2 decay (4 mV), markedly outperforming that of Pt/C (17 mV reduction). In related work, Cao et al. [114] successfully immobilized single-atom Co-N-C catalytic centers on helical carbon nanostructures (HCNTs), designated as Co-N-C@HCNT. Curvature-induced charge redistribution analysis revealed enhanced electron transfer between nitrogen and carbon atoms surrounding cobalt centers in the helical configuration, with peripheral carbon atoms demonstrating greater electron depletion and consequent charge concentration in catalytic zones. The modified Co-N-C@HCNT system displayed a downward-shifted d-band center (-1.34 eV versus -1.29 eV in planar counterparts), facilitating optimized adsorption-desorption energetics for reactive intermediates and consequent catalytic performance enhancement. The electrocatalytic performance of Co-N-C@HCNT demonstrates notable characteristics with a Eonset reaching 0.90 V versus RHE and a E1/2 of 0.86 V versus RHE, showing similarity to commercial Pt/C (20 wt%) catalysts, as illustrated in Fig. 10f. During prolonged stability testing over 10 h, the material maintained exceptional operational durability with only 4% current density attenuation (Fig. 10g). Comparative analysis reveals Co-N-C@HCNT's superior discharge power density at 130 mW/cm2, significantly outperforming the 96 mW/cm2 recorded for Pt/C + RuO2 hybrid systems (Fig. 10h), which highlights its enhanced catalytic efficiency and improved cycling performance in energy storage applications.

    To provide a overview of how different strain-inducing methods affect ORR performance, strain engineering strategies discussed above are summarized in Table 1, which compares five distinct strains and outlines the generation mechanism, typical catalyst examples, and the influence on ORR (including regulation range and activity metrics, such as MA and SA).

    Table 1

    Table 1.  Comparison of different strain.
    DownLoad: CSV
    Strain type Generation mechanism Typical catalyst Strain regulation range Influence on ORR activity References
    Strain of alloy structure Differences in atomic radii of mixed metals Pt56Mn44/C;
    Rh-Pt3Co/C;
    -0.43%;
    -2.9%
    MA = 0.53 A/mgPt
    SA = 1.0 mA/cm2;
    MA = 1.31 A/mgPt,
    SA = 1.77 mA/cm2;
    [66];
    [128]
    Strain of core-shell structure Lattice mismatch between core and shell Pt @Pt-skin Pt3Ni CSFWs;
    fct-PtCo @PtIr/C
    -4.9%;
    -1%~-3%
    MA = 6.69 A/mgPt
    SA = 8.42 mA/cm2;
    MA = 1.17 A/mgPt+Ir
    SA = 2.63 mA/cm2Pt+Ir
    [82];
    [79]
    Strain caused by the size and shape change Increased specific surface area of nanoparticles CS-Pt/C (2 nm);
    PtCoCu (2.98-10.9 nm)
    -0.5%~-2.5%;
    -2.38%~-2.84%
    MA = 1.72 A/mgPt
    SA = 0.99 mA/cm2;
    MA = 1.19 A/mgPt
    SA = 1.48 mA/cm2;
    [93];
    [129]
    Strain caused by defects Defects (vacancies, steps) Pt (21 21 20);
    the defective HOPG;
    -3.7% (step)
    -0.3% (terrace);
    +0.6%
    50 times (ORR improvement factor);
    35% (current density increased)
    [48];
    [194]
    Strain caused by the substrate Strong interactions at the metal-support interface Co-WC;
    BSPCFW
    -5%;
    +2%~+3%
    0.45 V (overpotential)
    E1/2 = 0.893 V vs. RHE;
    Rp = 0.068 Ω cm2 (600 ℃)
    [111];
    [228]

    Noble metal-based catalysts still domains in the commercial market because they are able to demonstrate efficient ORR catalytic performance. With the aim to enhance their utilization a wide variety of modifications have been conducted. At present, focuses are mainly concentrated on Pt, Pd, Ru, Au, and Ag containing catalysts. In this section, the strain engineering modification of several typical catalysts is introduced.

    Pt-based catalysts are the most widely employed electrocatalysts for ORR, owing to their ability to effectively lower the activation energy. The electrochemical catalytic performance of Pt-based catalyst for ORR is primarily attributed to the unique electronic structure of Pt, which facilitates optimal chemisorption of oxygen molecules [52,115-120]. Significant efforts have been devoted to developing catalysts with low platinum loading that can maintain long-term activity and stability, thereby addressing cost-efficiency concerns [121-123]. The Pt-based catalysts can be categorized into four distinct types, i.e., Pt/C catalysts, Pt-containing alloys, Pt-intermetallic compound, and core-shell catalysts. The strain effect exists in the alloy, intermetallic compound and core-shell structure formed by Pt and other metals, regulating the crystal surface and changing the surface electronic properties of these Pt-based catalyst. Nørskov et al. [124] established a fundamental theoretical framework correlating d-band center positioning with catalytic activity parameters. The electronic structure characteristics of Pt-based catalysts, particularly the d-band center position modulated through lattice strain effects, critically influence ORR performance. Consider the core-shell configuration as an illustrative case, when the atomic spacing parameters of shell elements measure smaller than those in the core material, surface atoms experience tensile strain. This structural distortion narrows the d-orbital bandwidth while shifting the d-band center upward toward the Fermi level. Such electronic state modification increases d-orbital vacancy density, thereby strengthening oxygen species adsorption. Conversely, compressive strain occurs when shell components possess larger lattice parameters than the core substrate, inducing downward d-band center displacement that weakens oxygen binding interactions [125,126]. These fundamental principles demonstrate that precisely engineering compressive/tensile strain fields to optimize Pt's d-band electronic configuration represents an effective strategy for enhancing the inherent ORR catalytic efficiency of platinum-based materials. In this section, the applications of strain regulated in Pt-based alloys, intermetallic compounds and core-shell catalysts are summarized in details.

    3.1.1   Pt-based alloy

    The high cost of Pt significantly restricts the large-scale application of Pt-based catalysts. Although the introduction of transition metals to form binary Pt alloys can effectively reduce material costs, these catalysts often encounter critical issues such as insufficient active sites (e.g., low activity in redox reactions) and stability degradation due to the dissolution of transition metals. To address this dilemma, researchers have developed ternary alloy systems that achieve synergistic effects through meticulously designed component ratios for electronic structure modulation and geometric effect coordination. This approach not only maintains cost advantages but also enhances catalytic activity and durability. In recent years, high-entropy alloy catalysts have demonstrated remarkable benefits due to their unique “cocktail effect” (multicomponent cooperative catalysis) and elevated configurational entropy (which suppresses element diffusion and phase separation) [127-137]. These characteristics provide an innovative direction for developing a new generation of economically viable Pt-based catalysts that exhibit both high activity and excellent stability. In the following, we will discuss three types of Pt-based alloy, namely, binary alloys, ternary alloys, and high-entropy alloys.

    Binary alloy: PtCo alloy is the most widely studied case in the family of Pt-based alloy. The introduction of compressive strain in PtCo alloy leads to a reduction in the d-band center of Pt due to the small atomic radius of Co. This results in a weakened adsorption of oxygen species, improving ORR activity. Additionally, Co and Pt can form highly alloyed and monodisperse nanoparticles. This structure exhibits better durability under acidic conditions and mitigates the dissolution of transition metals. According to the study of Nørskov [51], this structural modification generally lowers the d-band center of Pt, further diminishing the binding strength of oxygen intermediates, thus facilitating the acceleration of the ORR. Li et al. [127] prepared a family of carbon-supported PtCo alloy catalysts at different temperatures (PtCo/C), and the PtCo/C catalysts show excellent acid ORR electrocatalytic performance. It is found that due to the mismatch of the ionic radii of Co and Pt, local tetragonal distortion is induced and significant strain exists on the nanoparticle surface (Fig. 11b), which further shortened the Pt-Pt bond (Fig. 11a) and causes the downshift of d-band center of Pt (from -2.23 eV to -2.41 eV, Fig. 11c), thus weakening the adsorption of O intermediates and enhancing the performance of the catalyst. The kinetic current at 0.9 V for PtCo/C‐600 ℃ (jk = 40.5 mA/cm2) and its MA (2.27 A/mgPt) and SA (3.34 mA/cm2) are 8 times higher than that of Pt/C. As shown in Fig. 11d, after 30,000 ADT cycles, only 7.8% decrease in the power density (from 1.02 W/cm2 to 0.94 W/cm2) at a current density of 2 A/cm2 is found for PtCo/C‐600 ℃, which is less than that of the Pt/C catalyst with the same Pt loading (the peak power density decrease is ~20%).

    Figure 11

    Figure 11.  Strain in Pt-based alloys. (a) HR-TEM image of PtCo/C-600 ℃. (b) Variation of Pt-Pt bond lengths for different models along the (110) direction. (c) PDOSs and d-band centers of Pt (110) and models with localized strains. (d) Steady-state polarization curves after 30,000 cycles of ADT. Reproduced with permission [127]. Copyright 2024, Wiley-VCH. (e) ∆EO as a function of compressive strain on the (111) surface. The horizontal red line indicates the optimal value of ∆EO. (f) Comparative electrocatalytic metrics including MA and SA values at 0.9 V (vs. RHE) for S-PtCo SNPs/C, S-Pt3Co SNPs/C, and benchmark Pt/C catalyst. Reproduced with permission [55]. Copyright 2024, Springer. (g) Evolution of surface Pt d-band center during structural transformations. (h) Performance comparison of Pt-based catalysts (Pt/C, Pt3Co/C, Rh-Pt3Co/C) at 0.9 V operating potential. (i) Voltage stability assessment at 0.8 A/cm2 current density before and after electrochemical aging tests. Reproduced with permission [128]. Copyright 2024, Wiley-VCH.

    Tu et al. [55] developed strain-optimized Pt3Co solid-solution nanoparticles (designated as S-Pt3Co SNPs and S-PtCo SNPs) through precise cobalt content regulation in the alloy composition. Experimental data in Fig. 11e demonstrate that cobalt incorporation effectively modulates surface compressive strain, shifting the d-band center downward relative to pure platinum. This electronic structure modification facilitates oxygen molecule release from catalytic surfaces, thereby improving ORR efficiency. Performance metrics in Fig. 11f reveal S-PtCo SNPs/C achieves superior MA (0.79 A/mgPt) and SA (1.0 mA/cm2), surpassing both S-Pt3Co SNPs/C (0.44 A/mgPt, 0.74 mA/cm2) and conventional Pt/C catalysts (0.22 A/mgPt, 0.42 mA/cm2). The optimized S-PtCo SNP configuration enables remarkable energy device performance, delivering 2.08 W/cm2 power density in proton exchange membrane fuel cells at 4 A/cm2 current density, while zinc-air batteries achieve 143.1 mW/cm2 power output at 214.5 mA/cm2 operational current.

    To further enhance the performance of Pt3Co alloy, Liu et al. [128] proposed a Rh doping strategy to synthesis a Rh-Pt3Co/C catalyst by thermal diffusion method. The doping of Rh also induced compressive strain on the alloy surface. As shown in Fig. 11g, the compressive strain on the Rh-Pt3Co surface (-2.9%) is more negative than that on the Pt3Co surface (-2.2%), thereby weakening the adsorption energy of *OH and thus further improving the ORR activity. The MA and SA of Rh-Pt3Co/C (1.31 A/mgPt and 1.77 mA/cm2) are significantly higher than those of Pt/C (Fig. 11h). In addition, the compressive strain caused by Rh doping enhanced the interaction between surface and bulk phase atoms, increasing the vacancy formation energy of surface Pt atoms and the migration energy barrier of Co atoms. This is beneficial to inhibit the dissolution of Pt and the migration of Co, which ensures the structural stability of the alloy catalysts in the long-term electrochemical testing process. The durability test of the half-cell reveals that the catalyst MA decreased by only 8% compared to the initial after 170,000 potential cycles. Moreover, in the test of PEMFC single cell with very low cathode Pt load (0.05 mgPt/cm2), the peak power density maintains at 0.88 W/cm2 after 50,000 square wave scanning, and the voltage at 0.8 A/cm2 remains (Fig. 12i).

    Figure 12

    Figure 12.  Strain in ternary Pt alloys. (a) Correlation between Cu concentration and measured strain percentages obtained through XRD analysis and HRTEM visualization. (b) Comparative evaluation of nanoparticle dimensions calculated through XRD and TEM techniques across varying Cu compositions. (c) Interdependent relationships among ECSA, MA, SA, and lattice contraction effects relative to ternary alloy nanoparticle dimensions. Reproduced with permission [129]. Copyright 2023, Wiley-VCH. (d) Sequential fabrication steps for PtNiW/C catalyst production. (e) Atomic-resolution HAADF-STEM visualization with dimeric Ni-O-W coordination analysis through intensity profiling and two-dimensional strain distribution mapping via geometric phase analysis. (f) Corresponding K3-weighted magnitude of Fourier transform spectra from EXAFS. (g) PDOS of Pt-d orbitals in Pt foil, PtNi/C, PtW/C and PtNiW/C, including the ϵ values. (h) Mass activities at 0.9 V vs. RHE of four catalysts before stability (pure color) and after stability (gradient color). Reproduced with permission [130]. Copyright 2024, Wiley-VCH.

    Ternary alloy: In the ternary alloy system, a third metal is involved into the alloy. Wei et al. [129] further prepared a series of PtCoCu alloy catalysts with different size (2.98-10.9 nm) and compressive strain (2.38%-2.84%). As shown in Fig. 12a, the compressive strain obtained from XRD and TEM measurements are summarized, that is, 2.38%, 2.43%, 2.46%, 2.74%, 2.81%, and 2.84%, for Pt50Co33Cu17, Pt51Co27Cu22, Pt50Co26Cu24, Pt47Co26Cu27, Pt44Co24Cu32, and Pt42Co21Cu37, respectively, demonstrating copper content's critical role in modulating nanostructured alloys' lattice distortion. Particle size evolution exhibits non-linear behavior (Fig. 12b), with dimensions fluctuating between 2.8 nm and 11 nm as copper concentration increases. Compositional optimization yields preferred particle sizes within 3-6 nm, where surface coordination characteristics govern the available surface area (Fig. 12c). Notably, as Cu concentration rises, particle dimensions initially diminish before subsequently expanding, with detailed characterization confirming that alloy stoichiometry directly influences these structural parameters.

    Sun et al. [130] prepared carbon supported Ni-W dual-site modified Pt nanoparticles (PtNiW/C) by the atomic layer deposition (ALD) method (Fig. 12d). As shown in Fig. 12h, the compressive strain on PtNiW/C would increase from the inner subsurface to outmost surface. Through XAFS fitting (Fig. 12e), it is found that the bond lengths of Pt-Pt (2.72 Å) and Pt-O (1.68 Å) in NiW @Pt/C are shorter than those in Pt and PtO2 foils (~2.75 Å and ~1.8 Å, respectively), further indicating that the surface modification of Ni-W diatom produces compressive strain on the surface of Pt, thereby shortening the atomic spacing on the surface of Pt. This is consistent with the results of HAADF-STEM strain test (Fig. 12f). DFT calculations (Fig. 12g) indicate the d-band center were -1.85, -1.81, -1.95, -1.77 eV for Pt, PtNi/C, PtW/C and PtNiW/C, respectively, showing that the compressive strain pushes the d-band center closer to the Fermi level, optimizing the adsorption of O2 and improving the ORR performance. As shown in Fig. 12h, PtNiW/C exhibited good performance in both activity (the MA of 0.25 A/mgPt) and stability (only 6% activity loss after 4000 cycles CV), which is better performed than Pt/C (the MA of 0.127 A/mgPt and nearly 30% loss in activity after durability test).

    High-entropy alloy: In HEA catalysts, the mixture of multiple elements will increase lattice distortion, mainly resulting in compressive strain in Pt-based HEAs, which regulate the d-band center and weakening/strengthening the adsorption of oxygen intermediates and thereby enhancing the ORR performance [131-138]. Zhou et al. [135] used a machine learning-assisted strategy to design a Pt-HEA ORR catalyst. Surface strain (ξsurf, Fig. 13a) caused by lattice mismatch between the alloy core and the Pt shell in the HEA is evaluated from DFT calculations, which are taken as inputs by the ML model, and the crystal graph convolutional neural networks (CGCNN) model is utilized to accelerate the screening of Pt-HEA ORR catalysts. Among the structural-property data of 538 groups of PtM3 alloy screened by the CGCNN model, the study identified Pt (FeCoNiCu)3 as the optimal combination and prepared the Pt (FeCoNiCu)3 catalyst using the facile freeze-drying-thermal reduction method. As shown in Fig. 13b, the Pt (FeCoNiCu)3 catalyst exhibited MA (4.09 A/mgPt) and SA (7.92 mA/cm2) at 0.9 V. In addition, the E1/2 drop of this catalyst after 5000 cycles was only 11 mV, showing superior stability. Fig. 13c shows a positive correlation between SA and surface strain, confirming that εsurf is a good indicator of ORR activity. Zhang et al. [136] fabricated nitrogen-incorporated high-entropy alloy nanoparticles (N-Pt-HEA NPs) that induced compressive strain effects. This strain effect led to a reduction in the d-band center of Pt (-2.693 eV vs. -2.571 eV in undoped Pt-HEA), effectively weakening oxygen species adsorption and consequently enhancing oxygen electrocatalytic activity. Comparative durability tests in Figs. 13d and e revealed N-Pt-HEA NPs exhibited significantly improved stability during ORR operation compared to their non-doped counterparts, with the d-band center shift confirming the strain-mediated electronic structure modification through nitrogen incorporation. The Fermi level adjustment leads to diminished ΔE*O values, thereby reducing optimal ORR performance. N-Pt-HEA exhibits an extended Pt-O bond length of 2.080 Å compared to pure Pt (2.056 Å) and Pt-HEA (2.075 Å), further verifying its decreased ΔE*O. With a MA of 0.65 A/mgPt at 0.9V, N-Pt-HEA nanoparticles demonstrate 1.4-fold and 4.3-fold enhancements over Pt-HEA (0.46 A/mgPt) and commercial Pt/C (0.15 A/mgPt) respectively (Fig. 13e). Du et al. [137] synthesized a Pt-based HEA catalyst with a size of less than 3 nm by adjusting the polarity of the solvent and the interaction between the nanoparticles and the carrier, using ethanol and carbon oxide as precursors (E/O-PtFeCoNiMn/C). The catalyst exhibits a compressed lattice, and EXAFS data shows that the Pt-Pt bond length in E/O-PtFeCoNiMn/C is short (Fig. 13f), indicating lattice compression. As shown in Fig. 13g, compared with the d-band center of Pt (111) (-2.14 eV), the d-band center of E/O-PtFeCoNiMn/C (111) shifts upward (-1.67 eV), which helps to enhance the adsorption of O2, thus improving the activity of the electrocatalytic reaction. This electronic configuration advantage facilitates more efficient capture of small molecular species like H2O and O2, significantly accelerating electron transport mechanisms in ORR processes. Comparative electrochemical evaluations revealed that the engineered E/O-PtFeCoNiMn/C nanostructures exhibited substantially improved MA and SA for ORR when benchmarked against standard Pt/C catalysts, with detailed performance illustrated in Fig. 13h.

    Figure 13

    Figure 13.  Strain in Pt-based HEA. (a) The illustration of the surface strain (ɛsurf) originated from the lattice mismatch of the interface between the intermetallic/alloy core and Pt shell. The schematic illustration of the machine learning-guided element selection process toward low-Pt ORR catalysts. The area surrounded by the gray line represents the crystal graph convolutional neural networks (CGCNN) model. (b) Comparative catalytic performance metrics (mass/specific activity) measured at 0.9 V relative to RHE. (c) Correlation analysis between specific activity values and ɛsurf parameters. Reproduced with permission [135]. Copyright 2025, Wiley-VCH. (d) The calculated PDOS of Pt 5dz2 electrons. The gray, blue, and red lines stand for the d-band centers of pure Pt slab, Pt/HEA, and N/Pt/HEA, respectively. (e) Mass and specific activity (0.9 V vs. RHE) of N/Pt/HEA NPs-C, Pt/HEA NPs-C, and Com Pt-C catalysts. Reproduced with permission [136]. Copyright 2025, Elsevier. (f) EXAFS spectra of the E/O-PtFeCoNiMn/C catalyst and standard Pt foil in R-space. (g) The calculated DOS of Pt (111) and PtFeCoNiMn (111). (h) Calculated mass and specific activity at 0.9 V for ORR for E/O-PtFeCoNiMn/C and Pt/C catalysts. Reproduced with permission [137]. Copyright 2024, Elsevier.

    The “cocktail effect” (multi-element synergistic catalysis) of HEAs is strongly coupled with lattice distortion-induced strain effects, i.e., differences in atomic radii (0.124–0.139 nm) of different elements (e.g., Pt, Fe, Co, Ni, Cu) lead to a lattice distortion of 5%–8%, significantly higher than that of traditional binary alloys (2%–3%). EXAFS analysis of PtFeCoNiMn/C HEA shows that the Pt-Pt bond length shortens to 2.740 Å (compressive strain: 0.76%). Bader charge analysis reveals that Fe, Co, and Ni transfer 0.37–0.69 e to Pt, increasing the electron density on the Pt surface by 15% and enhancing O2 adsorption/activation [71,135]. Furthermore, adjusting the composition ratio of HEAs (e.g., Pt42Mn58) enables precise matching of strain and multi-element synergy. It is found that as Mn content increases, compressive strain rises from 0.36% to 0.76%, and the overlap between the 3d orbital of Mn and the π* orbital of O2 enhances, reducing the ORR energy barrier from 0.84 eV to 0.72 eV and increasing MA to 0.53 A/mgPt [66].

    3.1.2   Intermetallic compound

    Ordered intermetallic compounds exhibit definite stoichiometric ratio and provide better control over the geometric structure of metal atoms, thereby enabling the active centers to be uniformly distributed on the same surface and thus benefiting electrocatalytic activity [139-145]. For example, Wang et al. [139] prepared Pt3Co intermetallic compounds and found that the MA of L12-type ordered structure was 3.3 times that of disordered structure. Liang et al. [140] synthesized ordered PtFe intermetallic catalysts and found that there is a strong positive correlation between the ORR activity and the ordering degree. The highly ordered PtFe catalyst demonstrated a high SA of 2.12 A/mgPt in the tests of the rotating disc electrode and the H2-O2 fuel cell. In addition, compared with traditional PtM alloy, intermetallic compound exhibits higher thermal stability and chemical stability, which helps to maintain catalytic activity and structural integrity during long-term operation [146-150].

    The mechanism of strain-regulated Pt-based intermetallic compounds and PtM alloy in electrocatalytic ORR is similar. The compressive strain among them is introduced by doping other metals to reduce the d-band center of Pt, thereby weakening the adsorption of oxygen-containing intermediates and improving the performance of ORR. However, there are also some differences between them. The strain in PtM alloy is more difficult to control because of the disordered structure leads to an uneven strain distribution, which may accelerate the corrosion and performance degradation of the catalyst. On the contrary, the ordered structure of Pt-based intermetallic compounds can provide uniform strain, thereby precisely controlling the surface strain of Pt and improving the ORR performance. In particular, the ordered arrangement of atoms in intermetallic compounds makes their structure symmetrical, which is conducive to the precise control of strain and tune their catalytic performance [141-143]. For example, Hao et al. [143] fabricated two structurally distinct Pt3Ga intermetallics-Pt3Ga (Pm3/m) and Pt3Ga (P4/mbm)-along with a randomly arranged PtGa alloy to precisely tune compressive surface strain in platinum systems. Structural characterization revealed that in both intermetallic variants, gallium atoms preferentially located at the vertices of cubic unit cells while platinum atoms occupied the face-centered sites. Contrastingly, the PtGa alloy exhibited random atomic distribution within the face-centered cubic lattice, as verified through combined XRD analysis and HAADF imaging techniques (Fig. 14a). The Pt3Ga (P4/mbm) phase demonstrated reduced crystallographic symmetry compared to its Pm3m counterpart, featuring a quadratic rotational axis and mirror plane perpendicular to the a-c axes despite identical elemental composition. Experimental results demonstrated that the higher-symmetry Pt3Ga (Pm3m) variant achieved precise 2.7% lattice compression, effectively lowering the overpotential from 0.74 V to 0.56 V for ORR (Fig. 14b). This performance enhancement stems from optimized electronic structure modifications induced by controlled lattice contraction. As the d-orbital electrons of Pt became more populated, the d-band center associated with *OH adsorption shifted further from the Fermi level, resulting in reduced intermediate binding strength and enhanced catalytic kinetics (Fig. 14c). The structurally ordered Pt3Ga intermetallic phase (Pm3/m symmetry) demonstrated superior ORR performance with peak MA and SA values reaching 2.18 A/mgPt and 5.36 mA/cm2, respectively, surpassing commercial Pt/C and PtGa alloy catalysts by an order of magnitude in both metrics (Fig. 14d).

    Figure 14

    Figure 14.  Strain effects in platinum intermetallic compounds. (a) HAADF-STEM characterization of Pt3Ga (Pm3m) and Pt3Ga (P4/mbm) phases, with atomic structural models illustrating their orientation relative to the Pt (110) reference plane. (b) Correlation plot showing the interdependence of *O intermediate adsorption free energy, overpotential, and lattice compression characteristics on Pt surfaces. (c) Projected density of states analysis for Pt atoms bonded with *OH species in Pt3Ga (Pm3m). (d) Comparative evaluation of MA and SA at 0.9 V vs. RHE for PtGa alloys, Pt3Ga polymorphs, and commercial Pt/C catalysts. Reproduced with permission [143]. Copyright 2024, Wiley-VCH. (e) Atomic-resolution HAADF-STEM visualization of L10-Pt2CuGa nanoparticles, with inset fast Fourier transform pattern. (f) Comparative Pt L3-edge EXAFS Fourier transforms for L10-Pt2CuGa/C, L11-PtCu/C, and metallic Pt references. (g) Activity-structure relationship mapping between ORR specific activity and Pt-Pt bond distances. (h) Comparative analysis of vacancy formation energies for Pt (111) surfaces versus L10-Pt2CuGa systems. (i) ADT results showing ORR polarization curves for L10-Pt2CuGa/C before and after potential cycling. (j) Performance metrics tracking MA retention and hydrogen-oxygen fuel cell peak power output during stability assessments. Reproduced with permission [148]. Copyright 2024, Wiley-VCH. (k) Relation between strain, d-band center, and ORR free energy barrier of L10-GaPtCo, A1-PtCo, and Pt. (l) MA at 0.9 V in H2-O2 fuel cells and the voltage at 0.8 A/cm2 in H2-air fuel cells before and after AST test. Reproduced with permission [149]. Copyright 2023, Nature.

    Furthermore, in order to enhance the durability, L10-type chemically ordered intermetallic PtM (e.g., L10−PtM) have attracted wide attention [144,145]. Ordered intermetallic compounds exhibit stronger interatomic bonds than disordered counterparts. This is because the transition from disorder to order is usually accompanied with a decrease in enthalpy, which gives intermetallic compounds superior thermal stability [146,147]. Li et al. [148] introduced Ga into L11-PtCu, and stimulated a directional covalent atomic interaction between Pt and Ga, causing a phase transition from L11 to L10 in PtCu (Fig. 14e). The introduction of Ga is conducive to the transformation of PtCu intermetallic compounds from the L11 structure to the L10 structure (Fig. 14f), which effectively alleviates the excessive compression in the L11 structure, thereby optimizing surface oxygen adsorption through biaxial strain in the anisotropic lattice, and thereby promoting ORR activity. The oxygen adsorption energy (EO) on the surface of L10-GaPtCu/C plate increases linearly under surface compression. The SA and dPt-Pt of the studied catalyst is volcanically related (Fig. 14g) and it is found that the biaxial strain is 2%, the EO is 0.21 eV higher than that of Pt (111) plate, indicating that the EO value on the surface of L10-GaPtCu plate is optimal. Computational analysis reveals significantly elevated vacancy formation energy (Evac, defined as the energy needed to sever chemical bonds between surface Pt atoms and adjacent metal atoms), increasing from 0.98 eV in Pt (111) to 1.28 eV in L10-GaPtCu/C (Fig. 14h), confirming enhanced structural integrity and corrosion resistance. ADT conducted through 30,000 potential cycles (0.6-1.0 V vs. RHE) in oxygenated 0.1 mol/L HClO4 electrolyte (Fig. 14i) demonstrates exceptional stability, with merely 8 mV degradation in E1/2 while maintaining original morphology and elemental distribution. Following extended electrochemical cycling, the L10-ordered catalyst architecture demonstrated remarkable structural integrity. Proton exchange membrane fuel cell evaluations revealed that the L10-GaPtCu/C nanocomposite outperformed conventional Pt/C and L11-PtCu/C catalysts, achieving a mass activity of 0.57 A/mgPt at 0.9 V. The material exhibited exceptional performance metrics with peak power densities reaching 2.60 W/cm2 and 1.24 W/cm2 in hydrogen-oxygen and air-fed configurations respectively. Accelerated stress testing through 30,000 voltage cycles confirmed the catalyst's durability, retaining 85% of its initial mass activity and 92% of peak power output (Fig. 14j).

    Similarly, Liang et al. [149] developed a novel approach involving low-melting-point metal doping to fabricate structurally ordered L10-type M-incorporated PtCo intermetallic compounds (M = Ga, Pb, Sb, Cu). Using the Ga-doped L10-PtCo (Ga-PtCo) catalyst as a representative case, their investigation revealed a distinct relationship among lattice strain variations, d-band center positioning, and ORR energy barriers. Fig. 14k illustrates how progressive reduction in compressive strain across Pt, A1-PtCo, and L10-GaPtCo systems corresponds with systematic downward shifts in d-band center locations, consequently lowering free energy barriers sequentially. The L10-GaPtCo configuration displayed optimal characteristics with maximal compressive strain, minimal d-band center elevation, and superior ORR performance. As depicted in Fig. 14l, this catalyst demonstrated a mass activity of 1.07 A/mgPt at 0.9 V under H2-O2 fuel cell conditions and achieved a power density reaching 1.05 W/cm2 in H2-air configurations with platinum loading limited to 0.075 mg/cm2. After 30,000 cycles of AST, the L10-GaPtCo still maintained a high MA of 0.88 A/mgPt with a loss of 17.8%, which meets well the DOE stability target of less than 40% MA loss. The voltage loss of the MEA made with L10-GaPtCo was 27 mV at 0.8 A/cm2 after 30,000 AST cycles, also satisfying the DOE 2025 target (less than 30 mV).

    Cui et al. [150] developed a carbon-supported L10-type Pt0.8Ga0.2Co intermetallic compound catalyst (L10-Pt0.8Ga0.2Co/C) by partially replacing the Pt with Ga. DFT calculations indicated that the introduction of Ga can fine-tune the surface strain which approaches the optimal region of the theoretical volcano, accelerating ORR dynamics. The d-band center of Pt0.8Ga0.2Co (-2.20 eV) is negatively shifted compared with PtCo (-2.16 eV) due to the larger compressive strain in the e1 direction of Pt0.8Ga0.2Co, which produces weaker adsorption of oxygen-contained species for the doped case. Electrochemical testing demonstrated the optimized catalyst's superior performance, achieving 3.39 mA/cm2 intrinsic activity and 0.77 A/mgPt MA at 0.90 V under fuel cell operating conditions. Accelerated stress tests revealed exceptional stability with merely 28% MA degradation after 30,000 voltage cycles, significantly outperforming the Department of Energy's 40% degradation benchmark. This enhanced catalytic behavior stems from robust Pt-Ga covalent bonding that facilitates structural stabilization while optimizing surface electronic configurations.

    3.1.3   Core-shell structure

    By designing the core-shell structure, the utilization of Pt can be raised, which is particularly important for large-scale applications such as fuel cells that require a large amount of Pt. For example, in the core-shell structure, the core can be a low-cost metal or oxide, while the shell Pt is used to provide active sites. Moreover, the interfaces in the core-shell structure can provide extra active sites, which may act as the origin of the superior catalytic properties [151,152]. In addition, the core-shell structure can effectively prevent the dissolution of Pt in the core, thereby improving the durability of the catalyst [153,154].

    Kim et al. [153] constructed Pd@Pt nanocrystals (Pd@PtnL NCs, nL is the layer of Pt) featuring a core-shell structure through a rhombohedral dodecahedral synthesis technique. It was observed that the electrocatalytic activity of the Pd@Pt NCs towards the ORR diminished as their Pt shells became thinner which results in increased in-plane compressive surface strain. This finding stands in stark contrast to previous reports concerning Pt-based catalysts. Through DFT calculations, it was determined that the strain-active characteristics of the Pt (110) surface arise from the cancellation of outer plane surface strain and applied in-plane strain (Fig. 15a). The outer plane strain refers to the strain applied along the direction perpendicular to the Pt (110) plane. The applied in-plane surface strains along the [001] and [110] directions are summarized in Fig. 15a. Notably, Pd@Pt5-6L NCs exhibited compressive strains measuring 0.507% ± 0.112% and 0.509% ± 0.126% along both the [001] and [110] crystallographic axes respectively.

    Figure 15

    Figure 15.  Strain in Pt core-shell. (a) Surface strains of PdRD@Pt nL NCs along the two in-plane directions. (b) Specific and mass activities of different catalysts at 0.9 V vs. RHE. Reproduced with permission [153]. Copyright 2022, American Chemical Society. (c) Optimized configuration of Pt48Ag45Pb3 (111), Pt51Ag33Pb12 (110), and Pt55Ag19Pb22 (110) NCs image, (d) maps of the in-plan strain tensors εxx, εyy, εxy, processed via GPA taken from the yellow frame area. (e) PDOS for Pt and Pb atoms within Pt51Ag33Pb12 (110) and Pt55Ag19Pb22 (110) nanocrystal systems. Reproduced with permission [154]. Copyright 2022, Wiley-VCH. (f) Free energy profiles. (g) Correlation between tensile strain in platinum nanoparticles and incorporated nitrogen atom quantities. (h) MA variations across catalyst materials before and after 20,000 electrochemical cycles. Reproduced with permission [155]. Copyright 2020, Elsevier. (i) ORR enhancement (lower panel) and associated tensile strains (upper panel) relative to third-layer zirconium deposition thickness in Pt-shell configurations. Reproduced with permission [156]. Copyright 2019, American Chemical Society.

    Contractile strain is observed along specific crystallographic orientations when compared to the conventional Pt (110) surface configuration. Progressive thickening of the platinum shell leads to a gradual reduction in this strain phenomenon. Both Pd@Pt9L and Pd@Pt16L nanocatalysts displayed negligible compressive strain, suggesting substantial relief of interfacial strain between the Pt overlayer and Pd core through increased shell thickness. This structural evolution correlates with declining ORR performance in Pd@Pt nanostructures as Pt shell thickness decreases, where intensified in-plane compressive strain becomes evident (Fig. 15b). The catalytic performance of Pd@PtnL systems demonstrates strong dependence on Pt layer count, showing substantial enhancement in both SA and MA when atomic layers expand from 5-6 to 9. The observed MA reduction in Pd@Pt16L configurations stems from structural expansion effects. Current consensus maintains that core materials with smaller lattice parameters than platinum in core-shell architectures induce compressive surface strain, causing d-band center downshifting that improves ORR kinetics. This established strain-activity relationship appears inconsistent with certain experimental observations in these catalytic systems. Research data indicate that the alleviation of in-plane compressive strain on Pt (110) surfaces significantly improves ORR performance, contrasting with previous assumptions about strain-related activity reduction. The observed enhancement mechanism stems from modified surface electronic states rather than simple geometric strain effects.

    Mahmood et al. [154] synthesized ultra-thin PtPb layer around the PtAgPb, a core-shell nanoplates by oxidation-etched surface restraint packaging defects (Fig. 15c). Structural analysis using GPA strain mapping demonstrated predominant lattice contraction effects in PtAgPb nanoplates (Fig. 15d), with this compressive deformation modifying the electronic configuration of surface Pt atoms. The altered d-band characteristics reduced intermediate adsorption strength while enhancing catalytic performance (Fig. 15e). Compositional analysis via XRD revealed a descending silver content gradient across different crystal facets in the order of Pt48Ag45Pb3(111) (46.88%) > Pt51Ag33Pb12(110) (34.38%) > Pt55Ag19Pb22(110) (19.80%). As shown in Fig. 15f, the Pt55Ag19Pb22 (110) showed the lowest overpotential (0.47 V) compared with the Pt48Ag45Pb3 (111) and Pt51Ag33Pb12 (110), indicating efficient ORR activity of Pt55Ag19Pb22 (110) nanocrystal-based catalyst.

    As demonstrated, in most Pt-based catalysts, the compressive strain reduces the d-band center of Pt, weakening the adsorption of O intermediates and thus enhancing ORR activity. However, it has been shown that the introduction of tensile strain can also optimize the adsorption of O species to enhance ORR activity [155,156]. For example, Yang et al. [155] developed an N-doped Pt/C catalyst whereby the doping of N atom induces lattice tensile strain (Fig. 15g) The E1/2 of N-doped Pt NPs/C (0.927 V) exhibits a positive shift of approximately 6 mV relative to that of commercial Pt/C (0.921 V). As shown in Fig. 15h, N-doped Pt NPs/C exhibited the largest mass activity of 101.8 mA/mgPt at 0.90 V vs. RHE, which is 6.4% and 7.0% higher than those of N-doped Pt NPs/C single bond H2 (95.7 mA/mgPt) and commercial Pt/C (95.1 mA/mgPt), respectively. Kudo et al. [156] prepared Pt/Zr/Pt (111) structure composed of Pt (111) shell by alternately plating Zr and Pt on the surface of pure Pt (111) under UHV environment, and the average tensile strain of Pt (111) shell surface is less than 0.8% based on XRD analysis. Fig. 15i showed that 0.05% tensile-strained Pt/Zr/Pt (111) exhibits a maximum enhancement factor of 5 for the ORR activity, compared with Pt (111). This indicates that whether to introduce or what type of strain should be introduced has to be analyzed from case to case.

    As a sister compound to Pt, Pd shares analogous physicochemical properties and crystallographic structures. Notably, Pd boasts a relatively abundant presence in the Earth's reserves, positioning Pd-based catalysts as promising alternatives to their Pt-based counterparts. However, a significant challenge arises from the tendency of Pd surfaces to bind excessively to oxygen intermediates, resulting in substantially lower activity for the ORR compared to Pt. To address this limitation, various strategies have been employed to enhance the activity and durability of Pd catalysts [157-170]. The following part focuses on the modulation of strain in Pd-based alloys, as well as the exploration of core-shell and other advanced structural designs, paralleling the approaches used for Pt-based compounds.

    Alloying Pd with other transition metals (Au, Mo, Fe, Co, Ni, Cu, etc.) that introduces strain has also been widely studied [157-160]. Interestingly, unlike the compressive strain mechanism that enhances ORR efficiency in Pt-based alloys, Pd-M systems demonstrate improved performance through tensile strain effects that typically reduce oxygen species adsorption strength. A notable example involves Pd-Au bimetallic systems, where the larger atomic radius of gold (a = 4.079 Å) compared to palladium (a = 3.890 Å) generates structural distortion through lattice expansion when alloyed [157,158]. This phenomenon was experimentally verified in Pd-Au hollow nanospheres (PdAu HSs) developed by Che et al. [159], where cobalt nanoparticle templating enabled precise structural control. Geometric phase analysis revealed characteristic compression-tension dislocation patterns in Pd-Pd bonding networks (Figs. 16a1-a3, b1-b3), suggesting preferential strain localization around Au atomic cores. Notebly, the proportion of Pd/Au significantly influenced alterations in surface composition and structural characteristics. Fig. 16c shows composition-dependent surface strains, where more strain cores corresponding to the bond movements and rotations appeared as Pd/Au ratio decreased. Certainly, there existed residual lattice strain in the Pd HSs imposed by the structure with abundant of grain boundary. Particularly, visual evidence of the strain distribution of Pd6Au HSs and Pd3Au HSs demonstrated that both tensile strain and compressive strain are markedly more pronounced on the PdAu-skin compared to the Pd-skin. The ORR activities displayed a volcano type as a function of Pd/Au ratio (Fig. 16d). The Pd3Au HSs demonstrated a SA of 0.13 mA/cm2, surpassing the SA of Pd/C (0.05 mA/cm2) by a factor of 2.6. The MA measurements revealed Pd3Au HSs achieved 0.153 A/mgPd+Au, exhibiting a MA value 2.28-fold higher than of Pd/C (0.067 A/mgPd). These electrochemical enhancements highlight the superior catalytic efficiency of the hollow-structured Pd3Au system compared to conventional Pd/C catalysts.

    Figure 16

    Figure 16.  Strain in Pd-based alloys. (a) TEM images paired with dilatational strain distributions for (a1) Exx, (a2) Exy and (a3) rotational strain patterns observed in Pd6Au HSs. (b) Corresponding TEM visualizations with (b1) Exx, (b2) Exy strain mappings and (b3) rotational strain profiles for Pd3Au HSs. (c, d) Quantitative analysis showing strain center density (/nm2, exx) correlations with E1/2 in PdAu HSs. Reproduced with permission [159]. Copyright 2020, Elsevier. (e) Current-time profiles comparing electrochemical stability of Pd4Au HSs/C, Pd4Au HCs/C, and commercial Pt/C catalysts at 0.6 V versus RHE. (f) Performance metrics illustrating MA and SA comparisons at 0.85 V vs. RHE. (g) Schematic illustration of synthetic methodology for PdAu HCs. (h) TEM characterization of Pd4Au HCs with GPA-derived strain mappings. Color-coded dilatational strain (εxx) distributions (green-dark blue indicating compression, red-yellow representing tension) and rotational strain patterns. Reproduced with permission [160]. Copyright 2020, Wiley-VCH.

    Furthermore, one-dimensional hollow nanostructures are advantageous for enhancing both the activity and stability of ORR. The concave geometry of these structures generates pronounced local strain, which intensifies the accumulation of surface charge at the concave corners. This phenomenon facilitates the adsorption of oxygen-containing species, thereby promoting catalytic performance. Che et al. [160] synthesized a PdAu hollow nanochain (PdAu HCs) with one-dimensional architecture and ultra-thin Pd-rich films characterized by periodic concave structures, which confer a pronounced strain effect (Figs. 16g and h). The concave corner region produces stronger strain shells than the arc-edge region, and this substantial lattice strain can increase surface charge accumulation, which significantly influences surface electronic structure, thereby modulating the adsorption strength of intermediates on the Pd surface and then minimizing the coverage of unreactive oxygenate species to tailor the ORR performance. As illustrated in Fig. 16e, Pd4Au HCs demonstrated only a 12% decline in current density over a 20,000-s period, whereas the commercial Pt/C catalyst suffered a more substantial 28% decrease. The MA analysis revealed significant enhancement, with Pd4Au HCs achieving 0.287 A/mgPd, a remarkable 5.52-fold improvement compared to commercial Pd/C (0.052 A/mgPd, Fig. 16f). This substantial difference highlights the superior electrochemical stability and catalytic efficiency of the Pd4Au hybrid structures under prolonged operational conditions.

    Among the PdM alloy catalysts, PdMo alloy is another kind of ORR catalyst reported in literature [161,162]. Guo et al. [161] reported a highly curved PdMo alloy of sub-nanometer thickness in the form of metallic nanosheets, which exhibited highly efficient ORR activity in alkaline electrolytes (16.37 A/mgPd current density at 0.9 V vs. RHE). The MA was 78 and 327 times higher than that of the industrial Pt/C and Pd/C catalysts, respectively, with almost no decay after 30,000 cycles. The authors elucidated the origin of the enhanced ORR activity by DFT calculations. A four-atom layer model of PdMo bimetal was established as shown in Fig. 17a. ∆EO of PdMo bimetal is calculated as a function of biaxial strain (Fig. 17b) and it is found that ∆EO reaches the optimal value when the tensile strain is about 1%. In addition, there is a large amount of charge transferred from Mo to Pd (0.89 e per Mo atom) on the top and bottom surfaces. As shown in Fig. 17c, the transferred electrons fill the d-band (antibonding state) of the surface Pd atom, causing the d-band center to shift negatively by 0.26 eV relative to the pure four-layer Pd sheet. The downward shift of the d-band center eases the excessive binding of surface oxygen, promoting ∆EO to move toward the optimal value.

    Figure 17

    Figure 17.  Strain in PdMo alloys. (a) Left panel displays the lateral perspective of the nanoscale architecture in four-layered PdMo bimetallene. Right panel illustrates the planar configuration highlighting atomic arrangements in layers 2-3. (b) Variations in the ∆EO parameter for PdMo bimetallene under different mechanical loading conditions (compression vs. tension). A reference threshold value is marked by the crimson horizontal indicator. (c) PDOS analysis for surface Pd atoms across bulk palladium, four-layer Pd nanosheets (Pd 4L), and Pd-Mo composites. Dashed horizontal markers denote computed d-band central positions. Reproduced with permission [161]. Copyright 2019, Nature. (d) CV curve of PdMo recorded in a 0.1 mol/L HClO4 electrolyte. (e) Magnified image of the (111) diffraction peak as highlighted with a rectangle. (f) Micro-strain calculated from WAXS data using the W-H method. (g) Site-dependent PDOSs of Pd-4d and (h) Mo-4d orbitals in PdMo-H10m. (i) Adsorption energy and charge comparisons of *O2. (j) Reaction energy of the ORR under U = 0 V. (k) Comparison of SA and E1/2 for PdMo, PdMo-H10m, and PdMo-H. Reproduced with permission [163]. Copyright 2024, American Chemical Society.

    In another study, Li et al. [163] developed an electrochemical approach to regulate the micro-strain on the surface of PdMo nanoalloy electrocatalysts whereby the surface of Pd was treated by H absorption followed by its subsequent release (Fig. 17d). Fig. 17d shows the cyclic voltammetry curve recorded in 0.1 mol/L HClO4 solution over PdMo NCs in the potential window from -0.01 V to 0.40 V vs. RHE, in which several hydrogen related peaks. The PdMo-H10m, with H absorption time curves of 10 min, display an obvious broadening instead of a shift as compared with that of PdMo (Fig. 17e), suggesting the existing of strain, and this was verified by the measurement of Fig. 17f, whereby the PdMo-H10m exhibits severer strain value (ε = 2.26 × 10−1) than that of PdMo (ε = 1.03 × 10−1). Then, the site-dependent PDOSs of Pd 4d orbitals at different positions in PdMo-H10m are compared (Fig. 17g). In contrast to bulk metal Pd, the d-band center of Pd in PdMo-H10m is slightly downshifted, a consequence from the micro-strain. The 4d orbitals of Pd and Mo sites strongly overlapped in PdMo-H10m as compared to that in PdMo, which improves site-to-site electron transfer and enhance ORR activity (Figs. 17g and h). As shown in Fig. 17i, PdMo-H10m exhibited more negative adsorption energy than PdMo, which results in stronger O2 binding, facilitating the activation of the O2 and dissociation of the O-O bond during the ORR process. The average charge of adsorbed *O2 on PdMo-H10m is -0.48 e, larger than that on PdMo (-0.27 e). As shown in Fig. 17j (U = 0 V), the overall ORR process on both PdMo-H10m and PdMo display a downhill trend, and the PDS (*OOH → *O) requires an energy of 0.91 and 0.84 eV, respectively. The optimized PdMo alloy catalyst exhibits an ORR E1/2 of 0.929 V with a SA as high as 5.09 mA/cm2 at 0.9 V vs. RHE in an alkaline electrolyte, about 10.6 times that of the state-of-the-art Pt/C electro-catalyst (Fig. 17k).

    Ternary Pd-based catalysts are typically synthesized through the formation of alloy nanostructures composed of Pd, an additional transition metal (such as Fe, Co, Ni), and a third element (Pd, Bi, In, Sn, etc.) [164,165]. The incorporation of different elements induces lattice strain within the Pd matrix, which alters its electronic structure and optimizes the adsorption of oxygen species. Liu et al. [164] developed Pd@PdBiCo metallic aerogel (MAs) with tensile strain, which exhibits high ORR catalytic activity (Fig. 18a). The lattice spacing of the Pd@PdBiCo MAs is measured at 0.232 nm, marginally larger than that of Pd MAs (0.226 nm) (Figs. 18c-f), thereby confirming the presence of tensile strain in Pd@PdBiCo MAs. As far as the ORR activity is concerned (Fig. 18b), the E1/2 of Pd@PdBiCo MAs is 0.874 VRHE, representing an enhancement of 0.027 VRHE over Pd MAs and 0.048 VRHE over commercial Pd/C. The MA (1.034 A/mgPd) is 2.9 and 6.6 times higher than that of Pd MAs (0.351 A/mgPd) and commercial Pd/C (0.156 A/mgPd), respectively.

    Figure 18

    Figure 18.  Strain in Pd HEA. (a) Preparation of Pd@PdBiCo MAs. (b) Comparison of E1/2 and mass activity of the commercial Pd/C, Pd MAs/C, and Pd@PdBiCo MAs/C. (c) HRTEM images of Pd@PdBiCo MAs and (d) Pd MAs. (e) Integrated pixel intensified of Pd (111) lattices and (f) PXRD patterns of Pd@PdBiCo MAs and Pd MAs. Reproduced with permission [164]. Copyright 2023, Wiley-VCH. (g1) High-magnification TEM; (g2) FFT-derived crystallographic orientation; (g3) Strain mapping visualization; (g4) Quantitative strain measurement across particle diameter (compressive strain denoted by negative values) [166]. (h) Comparative strain analysis among PdCuMoNiCo NHSs, ternary/quaternary alloys, and pure Pd. (i) Normalized MA_SA at 0.8 V vs. RHE. Reproduced with permission [167]. Copyright 2022, Royal Society of Chemistry. (j) Catalytic performance benchmarking of 5-Pd-HECs/C against Pd-NCs/C and commercial Pt/C at 0.9 V vs. RHE. Reproduced with permission [166]. Copyright 2024, Royal Society of Chemistry.

    Pd based HEAs have also been documented in which Pd serves as the active center of the catalytic reaction, while other elements regulate the adsorption energy of the reaction intermediates and accelerate subsequent transformation. The introduction of heteroatoms typically introduces strain within the alloy structure. Hu et al. [167] prepared a Pd-based HEA by a simple solvothermal method, discovering that the hollow structure of the prepared Pd-based HEA alleviated the excessive strain caused by heteroatoms, resulting in excellent catalytic performance (Fig. 18h). Specifically, the MA of the PdCuMoNiCo HEA is 0.882 A/mgPd, which is 1.40 time of that of the commercial Pt/C (0.630 A/mgPt), and much higher than that of the as-synthesized Pd (0.092 A/mgPd), PdCu (0.417 A/mgPd), PdCuCo (0.421 A/mgPd), and PdCuNiCo (0.279 A/mgPd) (Fig. 18i). However, in another study, ORR activity was enhanced by the small size of the Pd-based HEA and the compressive strain in the alloy. Zhang et al. [166] synthesized homogeneous five-element PdMnFeCuNi HEA by a fast Joule heating method. The strain effect between Pd and other transition metals in PdMnFeCuNi HEA was confirmed by the strain profile and STEM diagram whereby the reduced interplanar spacing indicates the formation of Pd-based alloy phase and also demonstrates a certain lattice contraction in the cluster, arising ~2.6% compressive strain, because of a relatively higher atomic radius of Pd (0.137 nm) to Mn (0.132 nm), Fe (0.127 nm), Cu (0.128 nm), and Ni (0.124 nm) (Fig. 18g). In ORR, PdMnFeCuNi HEA showed 0.99 A/mgPd MA and 0.88 mA/cmPd2 SA, which are 4.95 and 2.44 times higher than those of commercial Pt/C, respectively (Fig. 18j).

    Pd metalene is a two-dimensional (2D) material characterized by its metal-like structure, comprising layers of Pd atoms. This material exhibits excellent properties in the field of catalysis attributed to its unique geometry. Through surface structure modification, strain effect and other strategies, the ORR catalytic activity and selectivity of Pd metalene can be significantly improved. Notably, Pd metalene with a concave surface can provide more stable active sites due to an increased coordination number, thereby improving the E1/2 to 0.947 V for ORR, along with remarkable cyclic stability [168]. Additionally, the tensile stress induced by the concave surface structure leads to an elongation of bond lengths, further optimizing catalytic activity [169].

    Sun et al. [170] prepared a 2D Pd nanomesh (Pd NM) which is characterized by overstretching the distance between the outermost crystal plane and the edge of the second layer of pores compared to the normal distance. Fig. 19a presents a typical edge of a nanopore along the Pd (200) planes, in which a significant expansion of the d-space from the inner 1.97-2.36 Å for the uttermost layer was identified. Furthermore, the GPA result of Area 1 shows a distinct distribution of lattice expansion along the direction of eyy. yet there was no expansion for Area 2 (the outer edge of nanomesh, Fig. 19b). In order to clarify the quantitative relationship between the strain and the ORR performance, Pd (200) facet under different expansion, i.e., Pd without strain (m1), those with the strains perpendicular to the Pd (200) facet of 5% (m2), 15% (m3), and 25% (m4) were examined (Fig. 19c). It is found that m4 is the closest to the peak of the limiting potential in the volcano plot. With the enlargement of expansion rate for m2 (5%) to m4 (25%), the reaction energy barrier of the RDS decreased from 0.919 eV to 0.825 eV, and then 0.781 eV. The d-band center shifted to negative energy by 0.038 eV (m2), 0.099 eV (m3), and 0.139 eV (m4), respectively, compared with m1, resulted by the d-band (the antibonding states) filling by the transferred electrons. The over-binding of oxygen on the surface is thus relieved (Fig. 19d). Consequently, the ORR catalytic activity of Pd nanomesh is greatly enhanced. At 0.9 VRHE, the MA is 2.672 A/mgPd, which is 27.8 and 23.6 times that of the commercial Pt/C and Pd/C catalysts, respectively. The SA of 1.704 A/cm2 is 6.3 and 5.4 times that of commercial Pt/C and Pd/C electrocatalysts, respectively (Fig. 19d). As shown in Fig. 19e, Pd NM/C exhibited improved current density (1.20 A/cm2) at 0.6 V and peak power density (Pmax, 0.86 W/cm2) at the beginning of life.

    Figure 19

    Figure 19.  Strain in Pd nanomesh. (a1) Magnified HAADF-STEM visualization of the perforation's interior margin (yellow frame). (a2) Cumulative intensity profiles across Pd (200) crystalline planes. (a3) Strain field mapping through geometric phase analysis (eyy component) corresponding to the zoomed Area 1. (b1) High-resolution HAADF-STEM examination of the mesh periphery (red frame). (b2) Integrated intensity distribution along Pd (111) crystallographic planes from Fig. 2f. (b3) GPA-derived strain mapping (eyy component) for Area 2, with chromatic scale indicating -20% to +20% strain variation. (c1) Surface structural configurations (m1-m4) in plan view. (c2) Catalytic activity profiles comparing *OH (black) and *OOH (green) adsorption energies for 4e− pathways. c3) Comparative d-orbital electronic structures with vertical markers indicating d-band center positions. (d) MA versus SA performance metrics at 0.9 V RHE. (e) Volumetric current density at 0.6 V and maximum power output characteristics. Reproduced with permission [170]. Copyright 2025, Wiley-VCH.

    The application of lattice strain engineering in noble metal-based catalysts for ORR extends beyond Pt, Pd to encompass Au, Ag, Ru, Rh, Ir, and other metals within their respective families [171-173]. For example, Guo et al. [174] prepared an excellent three-function catalyst (Ru/RuO2@NCS) by anchoring the lattice mismatched core/shell Ru/RuO2 NCs onto nitrogen-doped carbon nanosheets (Fig. 20a). The RuO2 shell comprising approximately 5 atomic layers eliminates the ligand effect and generates around 2% surface compressive strain (Figs. 20b and c). Specifically, the RuO2 shell experiences a compressive strain of approximately 2% while the Ru core exhibits about 1.3% tensile strain. The compressive strain of RuO2 shell effectively reduces the reaction barrier and improves the binding affinity of rate-limiting intermediates (*OH, *O, *OOH, *H), increasing catalytic activity and stability. As shown in Fig. 20d, compared to the original surface model, the a-axial compressed models show a significantly enhanced ability to capture oxygen, with a corresponding reduction in the adsorption free energy of 2*O could also get a relatively lower energy. Thus, the compressive strain in both a-axis and biaxial direction promotes the dissociation and adsorption of O2, which directly accelerates the reduction process to water. To investigate the electronic structure of the core-shell system, PDOS calculations were carried out by constructing the heterojunction model comprising Ru and RuO2 (Figs. 20e and f). The results reveal a pronounced upshift of the d-band center of Ru in the RuO2 surface upon interaction with Ru, attributable to the electron transfer from Ru to RuO2. This interaction strengthens the intermediate binding of intermediates and enhances the catalytic activity. As shown in Fig. 20g, the Eonset of Ru/RuO2@NCS is 0.92 V. The E1/2 is 0.84 V, and the Ru/RuO2@NCS also shows negligible activity decay and without obvious structure and composition changing after 3000 cycles durability test (Fig. 20h).

    Figure 20

    Figure 20.  Strain in other noble metal catalysts. (a) Schematic illustration depicting the strained RuO2 structure. (b) XANES spectra at the Ru K-edge and (c) Fourier-transformed EXAFS spectra derived from k2-weighted data for Ru/RuO2@NCS, RuO2, and metallic Ru references. (d) Correlation between lattice strain in RuO2 and adsorption free energy of 2*O species. Electronic structure comparison through PDOS analysis for (e) unmodified RuO2 and (f) strain-engineered RuO2. (g) Electrochemical characterization showing ORR Tafel plots, limiting-current densities, and E1/2. (h) ORR durability test. Reproduced with permission [174]. Copyright 2022, Wiley-VCH. (i) Diagram for tailoring atomic strain of Fe sites by second metal atoms. (j) Fe Mossbauer spectrum of Ru/Fe-N-C. (k) Bar chart showing Eonset and E1/2 of Ru /Fe-N-C and the kinetic current density at 0.85 and 0.8 V. Reproduced with permission [175]. Copyright 2024, Elsevier.

    Researchers have synthesized a series of diatomic catalysts comprising Ru and various transition metals, including Fe, Co, Ni, Cu. These diatomic systems leverage synergistic and strain effect to regulate the electronic structure, thereby optimizing their ORR performance. For instance, Yin et al. [175] synthesized a Ru/Fe-N-C catalyst that utilizes the synergistic effect of diatoms to induce atomic strain. As depicted in Fig. 20i, a local tensile strain of 2.1% at Fe site was adjusted by the introduction of Ru. Furthermore, Fig. 20j illustrates that moderate tensile strain increases the population of electrons in the antibonding orbital of Fe-Ru diatoms, accelerating the reaction kinetics. Ru/Fe-N-C catalyst showed exceptional ORR activity in oxygen-saturated 0.1 mol/L HClO4 solution, with an initial potential of 1.020 V and a E1/2 of 0.860 V (Fig. 20k). Moreover, the compressive strain by the lattice contraction in Ru-Pt alloys, attributed by the smaller atomic radius of Ru, has been shown to elevate the d-band center of the metal site, enhancing the adsorption and dissociation capacity of O2. In the context of Ru based HEAs, such as RuFeCoNiMn-HEA [176], the synergistic interaction between Ru and other transition metals create local strains through lattice distortion, effectively optimizing the adsorption of intermediates.

    Introducing lattice distortion via microstructural imperfections or dopant integration emerges as a promising approach for fabricating superior-performance catalytic materials. As two-dimensional structural irregularities, grain boundaries (GBs) can generate localized crystalline deformation and atomic-level surface irregularities, creating distinctive reactive centers for electrochemical processes like the two-electron ORR [177-180]. Researchers led by Wang [180] developed high-energy interfacial gold nanoarrays demonstrating enhanced 2e− ORR performance and elevated hydrogen peroxide selectivity through precise control of GB concentration and interparticle stress gradients, categorizing them into low, medium, and high GB density configurations (designated L-Au NAs, M-Au NAs, and H-Au NAs correspondingly). High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) analysis revealed the crystalline architecture and strain patterns in H-Au NAs (Fig. 21a). The H-Au NAs structure comprises interconnected gold nanocrystals functioning as fundamental nanoparticle units, bridged by numerous GB interfaces. These interfaces not only reinforce structural integrity but also reduce surface and interfacial energies through optimized atomic arrangements. As shown in Fig. 21b, high-energy grain boundaries (e.g., ∑9 and ∑27 configurations, Fig. 20a) and triple junction networks create localized strain fields near defect surface terminations. These configurations generate strain-concentrated zones adjacent to structural imperfections, potentially enhancing adsorption energetics for reactive intermediates. Experimental data in Figs. 21c and d reveals a proportional correlation between GB concentration and lattice distortion magnitude. EXAFS characterization shows progressive lattice expansion values of ~2%, 4%, and 6% for L-Au NAs, M-Au NAs, and H-Au NAs respectively. Coordination number analysis demonstrates a decreasing trend across the series: Au nanoparticles (approximately 12), L-Au NAs (~10.9), M-Au NAs (~9.9), and H-Au NAs (~8.7). Through analyzing the relationship between GB density and catalytic performance, it is shown that the high GB density, extended lattice and low coordination number of H-Au NAs are the key factors for their excellent performance (Figs. 21e and f).

    Figure 21

    Figure 21.  Strain in Au/Ag-based catalysts. (a) High resolution HAADF-STEM micrograph of the GBs between the Au NP building blocks within H-Au NAs. (b) Real space strain maps along the x (εxx), y (εyy) and xy (εxy) directions. (c) Relationship between gas flow rates and GB surface density. (d) Correlation between GB surface density and lattice expansion/coordination number calculated from the Fourier-transformed EXAFS spectra. (e) Calculated H2O2 selectivity during potential sweep. (f) Correlation between GB density and the 2e− ORR activity, including onset potential, H2O2 selectivity, specific activity, and mass activity. Reproduced with permission [180]. Copyright 2024, Nature. (g) Raman spectra of Ag2Mo2O7 samples. (h) Electron localization function on (020) and (1¯02) planes of AMO2. (i) Shift of Mo d-band center, Ag d-band center, and O p-band center after coordination rearrangement. (j) PDOS of Mo 4d and O 2p orbitals. (k) PDOS of Ag 4d orbitals. Reproduced with permission [181]. Copyright 2024, Wiley-VCH.

    Dang et al. [181] reported a Ag2Mo2O7 catalyst with improved ORR reaction kinetics by in-plane strain. The Ag2Mo2O7 samples synthesized at the pH values of 2, 5, and 6 were designated as AMO1, AMO2, and AMO3, respectively. As seen from Fig. 21g which is the Raman spectra of the Ag2Mo2O7 samples, the MoO6 symmetric stretching shifted to a lower wave number and an additional vibration peak at 825.11 cm−1 was observed for AMO2, indicating tensile stress and lattice distortion in AMO2. From the Bader charge analysis, it can be seen that the (020) plane displayed more charge transfer from Mo sites to O sites due to the shorter Mo-O bonds in the distorted [MoO6]. The electron localization function (ELF) maps (Fig. 21h) suggests that electrons from the (020) plane are more delocalized and uniformly distributed due to the homogeneous lattice strain. This is conducive to the electron transfer between the substrate and adsorbates. As shown in Figs. 20i-k, the d-band center of Ag 4d on the (020) plane increased from -1.774 eV to -1.698 eV, the slightly upward-shifting Ag d-band center of (020) plane would influence slightly the adsorption strength of the adsorbates. While the d-band center of Mo 4d and the p-band center of O 2p decreased from -0.552 and -1.760 eV to -0.848 and -1.964 eV, respectively, demonstrating better d-p coupling. And the downward-shifting Mo d-band center in distorted octahedron on the (020) plane would weaken the strong interaction with catalytic reactants and accelerate the desorption process of catalytic reactants. Therefore, the lengthening of Ag-O bonds and the compression of Mo-O bonds in the (020) plane of Ag2Mo2O7 lead to d-band splitting and d-band center optimization, improving the adsorption behavior of the catalytic reactants and increasing the ORR activity.

    In contrast to precious metal catalysts such as Pt/C, non-precious metal catalysts primarily consist of transition metals such as Fe, Co, Mn, which are both abundant in the Earth's crust and relatively inexpensive [182-185]. Non-noble metal catalysts refer to catalysts without noble metals (Pt, Pd, Au, Ru, Rh, Ir), including metal-free carbon-based catalysts and transition metal (Fe, Co, Ni, Mn)-based catalysts (e.g., M-N-C, transition metal oxides/nitrides). This abundance renders them more economically feasible for large-scale industrial applications. However, the ORR activity of non-noble metal catalysts remains suboptimal. Although certain transition metal-based materials [186,187], have demonstrated ORR activities approaching or even exceeding that of Pt/C, the overall catalytic performance of non-noble metal catalysts still requires significant enhancement. Moreover, the long-term stability of these catalysts is often compromised by issues such as carbon corrosion at the active sites and the dissolution or desorption of metal ions during the catalytic process, which can lead to diminished activity over time. Non-noble metal catalysts encompass a diverse range of materials, including carbon-based metal-free catalysts, nitrogen-doped carbon-supported transition metal systems, as well as transition metal nitrides and oxides. In particular, the catalytic performance of nitrogen-doped carbon supported transition metal materials (M-N-C) can be optimized by adjusting the carbon substrate, metal type and coordination environment [188,189]. The structural flexibility enables precise adjustment of catalyst activity and selectivity through experimental design and theoretical calculations. As research progresses, the performance of non-precious metal catalysts continues to improve. Strain engineering can be identified as a pivotal approach to significantly enhance the ORR activity of these catalysts by modifying their electronic structure and geometric structure, as substantiated by theoretical calculations and experimental verification [190]. By precisely controlling the strain, such as introducing intrinsic defects or regulating surface curvature, non-noble metal catalysts with superior ORR activity and stability can be strategically designed.

    Metal-free carbon-based nanomaterials (CNMs), Such as graphene, carbon nanotubes (CNTs) and fullerene (C60), have been widely studied as potential substitutes for commercial precious metal catalysts due to their advantages of low cost, high structural regulation and good stability [191]. The strain effect, originating from bending structure and introducing defects, can weaken the intermediate adsorption and accelerate the electron transfer to enhance ORR activity [192].

    For high-curvature carbon nanoribbons (CNRs-C), DFT calculations show that tensile strain (1.5%) induced by curvature increases the charge density of C-C bonds near edge graphite N by 0.05 e/Å3 and enhances spin polarization by 30%, significantly promoting orbital overlap between the π* orbital of O2 and the p orbital of C atoms. This reduces the O2 adsorption energy from -0.41 eV to -0.68 eV, accelerating O2 activation [190]. For oxidized carbon nanotubes (o-CNTs), strain in 8 nm-diameter tubes reduces the bond order of C-O bonds from 1.0 to 0.85. Bader charge analysis shows that O atom acquires 0.12 e, enhancing the stability of *OOH intermediates and increasing H2O2 selectivity to > 90% [193].

    Zhang et al. [190] introduced the strain effect on the active C-C bond near the edge graphite N, which tunes the appropriate spin polarization and charge density of the carbon active center and this is kinetically conducive to the adsorption of O2 and the activation of O-containing intermediates (Fig. 22a). The constructed high-curved edge metal-free carbon nanoribbons (CNRs-C) E1/2 are 0.78 and 0.9 V at 0.5 mol/L H2SO4 and 0.1 mol/L KOH, respectively, which exceeded the ORR activity of flat carbon nanoribbons (0.52 and 0.81 V) and N-doped carbon sheets (0.41 and 0.71 V). Especially, the kinetic energy current density (JK) in acidic media is 18 times higher than that of flat carbon and N-doped carbon (Figs. 22b and c).

    Figure 22

    Figure 22.  Strain in metal-free carbon catalyst. (a) Structural comparison between P-A-GN and C-A-GN configurations, visualized using an iso-surface value of 0.0005 e/Å3. (b) Electrochemical characterization showing Tafel plot variations and (c) ORR polarization curves (1600 rpm) for CNRs-C samples under O2-saturated 0.1 mol/L KOH before and after 10,000 stability cycles. Reproduced with permission [190]. Copyright 2023, Wiley-VCH. (d) Experimentally determined structural parameters including C-O bond distances and C-O-C angular configurations. (e) Schematic representation of curvature-modified carbon surfaces. (f) Charge redistribution patterns visualized through differential density analysis (yellow: electron accumulation; cyan: depletion; iso-surface = 0.005 e/Bohr3). (g) Correlation between the Bader charges at the two neighboring C atoms and the O atoms and the C p-band center to R. (h) Performance comparison with recent reports. Reproduced with permission [193]. Copyright 2024, American Chemical Society. (i) Half Violin plots of overpotential for SWG-O sites. (j) Correlation between tensile strain and ORR current density at 0.05 V vs. RHE. (k) Structures of graphene models with various defects, MVG, DVG, and SWG. MVG, DVG, and SWG refer to the graphene nanoribbon with a monovacancy, divacancy, and Stone-Wales defect, respectively. (l) ORR polarization curves of pristine HOPG under different tensile strains ε from 0.0% to ~ 2.1%. (m) ORR polarization curves of D-HOPG under different tensile strains ε from 0.0% to ~ 2.4%. Reproduced with permission [194]. Copyright 2025, American Chemical Society.

    Li et al. [193] reported the dependence of the curvature for the o-CNT catalyst on the ORR activity (Figs. 22d and e). The computational model shows that curvature can change the geometry of the epoxy groups and exert greater strain on the C-O bonds in o-CNTs with smaller diameters, resulting in increased activity (Figs. 22f and g). This theoretical prediction was further supported experimentally with five o-CNTs with different diameters but similar oxygen-containing groups. The smallest diameter o-CNT (8 nm) provided the highest H2O2 FE ( > 85%, or molar selectivity > 90%) and MA (161 A/g) at 0.65 volts (Fig. 22h).

    In addition, the introduction of specific defects in carbon materials can similarly produce strain effect. Zhang et al. [194] used highly oriented pyrolytic graphite (HOPG) as a model catalyst and established a platform for continuously applying strain while collecting electrochemical signals. They established experimentally and theoretically the relationship between the tensile strain and its ORR activation effect (Figs. 22i-k). It is found that there is a weak negative correlation between the tensile strain and the ORR performance of the original HOPG film in the range of -1.0% to 2.0% strain, and the ORR performance was only improved by 9.7% by applying a compressive strain of about -0.8% (Fig. 22l). In contrast, for the defective HOPG film, the current density significantly surges by about 35.0% when a tensile strain of about 0.6% is applied to the surface. Combining experimental and theoretical analyses, it is found that sites with initially low activity, such as Stone-Wales defects, can be activated by applying a tensile strain of about 0.5%, thereby lowering the reaction energy barrier and altering the RDS (Fig. 22m). This study elucidated the effect of the intrinsic strain of carbon-based metal-free catalysts (C-MFCs) on the electrochemical catalytic performance, laid a solid foundation for the mechanistic understanding of complex catalytic reactions.

    In recent years, M-N-C catalysts have garnered significant research attention due to their exceptional catalytic activity and well-defined composition of active centers, positioning them as promising alternative to noble metal catalysts [195-197]. Various transition metals, including Fe [186], Co [187], Ni [198], Mn [199], have been extensively investigated in this field, yielding substantial advancements in our understanding of these materials. Among these, SACs, particularly those based on Fe-N-C, exhibit remarkable ORR catalytic activity under acidic conditions, with its intrinsic performance closely approaching that of commercial Pt/C, achieving an E1/2 of more than 0.85 V in acidic media [200]. However, under acidic conditions, Fe2+ ions can readily dissolve at the metal site of Fe-N-C catalyst and subsequently react with H2O2, a by-product of ORR reaction, via the Fenton reaction. The active free radicals generated during this process can compromise the integrity of the proton exchange membrane, resulting in a rapid weakening of catalytic activity and battery performance. In severe cases, this may precipitate faults such as short circuit of the battery [201]. Strain engineering offers a powerful method for enhancing catalyst stability by modulating the distribution and density of surfaced active sites, effectively adjusting the geometry and electronic structure of the catalyst. Through the precise regulation of strain, it is anticipated that the inherent trade-off between activity and stability in M-N-C catalysts can be overcome, facilitating the design of efficient and stable ORR catalysts.

    By utilizing graphene's distinctive property of negative thermal expansion, researchers can strategically design strained carbon-based support structures with enhanced efficacy [202-204]. Through high-temperature pyrolysis of ZIF-8 precursors to create nitrogen-enriched carbon matrices, Wu's team [205] successfully fabricated multiple single-atom catalysts displaying varied substrate curvature and metal-nitrogen bond distances. Their investigation revealed temperature-dependent relationships between Fe-N coordination characteristics and the catalytic performance/stability of Fe-N4 moieties during thermal treatment processes. Controlled pyrolysis temperatures induced measurable compressive strain effects on the carbon framework, systematically decreasing M-N coordination lengths. For example, thermal activation at 700 ℃ yielded the ZIF-NC-0.5Fe-700, which exhibited an increased pre-edge intensity (Fig. 23a), an indication of a reduction in symmetry around the Fe atoms or shorter Fe-N bond lengths in the Fe-N4 configuration. As the activation temperature increases, the carbon layer embedded by the Fe-N4 site undergoes out-of-plane ripples, resulting in local compressive strain in these Fe-N bonds (Fig. 23b). The activation energy of O-O bond breaking at FeN4 site with compressive Fe-N bond is low, which is kinetically favorable for ORR. The compression of the Fe-N bond also leads to a positive shift of the 3d orbital of Fe and a clear charge transfer of Fe to neighboring N, which favors oxygen adsorption at the FeN4 site (Fig. 23c).

    Figure 23

    Figure 23.  Strain in M-N-C catalysts. (a) XANES spectra of different catalysts. (b) Structural configurations and electron density distributions in FeN4 active sites under both relaxed conditions and 2% Fe-N bond contraction scenarios. (c) Electronic state analysis through Fe 3d orbital density of states for contrasting FeN4 configurations. Reproduced with permission [205]. Copyright 2019, Wiley-VCH. (d) Design schematic illustrating the FeCoNP@FeSA-N/C composite catalyst architecture. (e) Comparative free energy profiles and reaction pathways for catalytic processes, with RDS clearly identified. Reproduced with permission [206]. Copyright 2022, Wiley-VCH. (f) Durability assessment showing performance evolution of Fe-N-C catalysts under accelerated stress testing (30,000 AST cycles) across varied atmospheric conditions. (g) Synthetic strategy visualization for creating S1/S2 active sites through controlled pyrolysis environments. (h) Real-space (R-space) Fourier transforms of EXAFS data. (i) Reciprocal space (κ-space) EXAFS fitting comparisons for Fe-N-C-Ar, Fe-N-C-10%FG, and iron phthalocyanine references. Reproduced with permission [207]. Copyright 2023, Nature.

    Liu et al. [206] designed a cross-layer "facet strain strategy" to enhance the inherent activity of the FeN4 site by coating FeCo NPs (FeCo@Fe-N-C, Fig. 23d). In the prepared composite catalyst, FeCo (110) can reconstruct the FeN4 site on the motile sublayer through interlayer transferable compressive strain, thus optimizing geometric and electronic configuration of the reaction center. The FeCo@Fe-N-C revealed lower overpotential of 0.720 V than 1.138 V of the primitive one, indicating an easier process during RDS (Fig. 23e). However, this contact mode can only be optimized for part of the iron sites in the Fe-N-C catalyst due to limited coordination in unsaturated spaces. It inevitably leads to the defects of low load and poor stability of Fe-N-C. Wu et al. [207] used Fe2O3@ZIF-8 composite precursor as raw material (Fig. 23g) and introduced hydrogen as forming gas for thermal activation to prepare Fe-N-C catalyst (Fe-N-C-FG). The use of pyrolysis precursors under an inert atmosphere (for example, N2 or Ar) has long been the prevailing approach for forming FeN4 active sites in Fe-N-C catalysts (Fe-N-C-Ar) [208]. An FeN4C12 moiety contains pyrrolic N ligations, often denoted S1 sites. The other FeN4C10 moiety with pyridinic N environments is denoted the S2 site [209]. X-ray absorption near-side structure analysis showed (Figs. 23h and i) that the Fe-N bond length of Fe-N-C-FG catalyst was significantly shortened (1.95 Å) compared with the Fe-N bond length of Fe-N-C-Ar (2.02 Å), which improved the intrinsic stability and activity of FeN4 site. As shown in Fig. 23f, the Fe-N-C-FG catalyst exhibited the highest activity at the end of the AST, with an E1/2 of 0.83 V, close to the initial E1/2 of the Fe-N-C-Ar catalyst. The ORR activity of the Fe-N-C-FG catalyst stabilized after 5000 potential cycles, suggesting the existence of active sites with intrinsic stability. In contrast, the Fe-N-C-Ar continuously lost activity throughout the 30,000 cycles during the AST. The Fe-N-C-FG catalyst in membrane electrode assemblies maintains a current density of 67 mA/cm2 at 0.8 V (H2-air) after 30,000 voltage cycles (0.60-0.95 V under H2-air).

    Wu and colleagues [210] fabricated helical carbon architectures with three-dimensional curvature through pyrolysis of self-organized chiral surfactant-directed polypyrrole templates (Fig. 24a). The induced lattice distortion at compressed FeN4 active centers (1.5% bond contraction, Fig. 24b) modifies electronic configuration, notably downshifting the d-band center relative to planar counterparts. This electronic modulation reduces adsorption strength of oxygen intermediates, effectively lowering the oxygen reduction overpotential. This synergistic configuration leverages both metallic nanoparticle conductivity and single-atom catalytic efficiency, while the coiled architecture enhances mass transfer through its tortuous surface topography. The experimental results show (Fig. 24c) that the dynamic current density of the curved FeN4 site is as high as 7.922 mA/cm2 when the voltage is 0.9V in alkaline medium, which is 31 times that of the planar FeN4 site. The catalytic behavior of FeNS/Fe3C@CNS can be controlled through mechanical stress arising from its distinctive helical nanostructure with pronounced curvature (Fig. 24d) [211]. Demonstrating exceptional performance in ORR, this composite material achieves a E1/2 of 0.91 V in alkaline environments and 0.78 V under acidic conditions. Kinetic analysis reveals a Tafel slope value of 106 mV/dec for FeNS/Fe3C@CNS (Fig. 24e), confirming accelerated reaction dynamics during ORR processes. Stability testing in oxygenated 0.1 mol/L HClO4 at 0.66 V versus RHE showed the catalyst maintains 85% initial current density after 10 h continuous operation (Fig. 24f), underscoring its durable electrocatalytic functionality.

    Figure 24

    Figure 24.  Strain in curved M-N-C catalysts. (a) Fabrication procedure for D-Fe SAC. (b) EXAFS analysis outcomes comparing D-Fe SAC with LD-Fe SAC. (c) Electrochemical performance metrics including E1/2 and kinetic current densities (0.9 V vs. RHE) across catalyst variants. Reproduced with permission [210]. Copyright 2021, Wiley-VCH. (d) Schematic representation depicting the synthesis pathway for FeNS/Fe3C@CNS. (e) Comparative Tafel slope measurements among FeNS/Fe3C@CNS, FeN/Fe3C@CNS, CNS, CNT@Fe and Pt/C in 0.1 mol/L HClO4 electrolyte under O2 saturation. (f) Chronoamperometric stability profiles of FeNS/Fe3C@CNS versus Pt/C in acidic media. Reproduced with permission [211]. Copyright 2024, Wiley-VCH. (g) Preparation methodology illustration for FePc-{PW12}@NT and FePc-{PW12}/NT catalytic systems. (h) Electron density distribution patterns in FePc-NT versus FePc-{PW12}@NT (isosurface level: 0.0005). (i) Comparative free energy profiles for ORR mechanisms across FePc-{PW12}@NT, FePc-NT and FePc configurations. (j) Catalytic activity indicators showing kinetic current densities (JK) at 0.8 V and corresponding E1/2. Reproduced with permission [212]. Copyright 2023, Wiley-VCH.

    Iron phthalocyanine (FePc) with a FeN4 active center exhibits weak adsorption of O2 by planar symmetric molecules. Strain engineering can break the structural symmetry and improve the ORR performance of FePc-based catalysts [113]. Zhu et al. [212] synthesized polyacid carbon nanotube clusters with one-dimensional heterogeneous structure and used them as carriers to support FePc molecules (FePc-{PW12}@NT, Fig. 24g). The curvature effect of carbon phosphor-tungstic acid nanotubes causes biaxial strain of iron phthalocyanine molecules, breaking the symmetry of the planar structure and enhancing the ORR performance. Fig. 24h illustrates how the encapsulation of {PW12} clusters within single-walled CNTs generates localized tensile strain, which subsequently modifies the molecular geometry of FePc and stabilizes the composite architecture. These structural modifications and electron localization enable precise adjustment of the electronic configuration for Fe and spatial charge distribution, ultimately optimizing the ORR catalytic behavior through tailored coordination environments. The catalytic performance of the FeN4 active site was investigated through comparative analysis. As illustrated in Fig. 24i, the FePc-{PW12}@NT catalyst demonstrates a reduced activation energy barrier of 0.45 eV compared to pristine FePc (0.51 eV). This one-dimensional heterostructured molecular catalyst displays outstanding ORR catalytic performance, achieving a E1/2 of 0.9 V that notably exceeds the 0.85 V value recorded for Pt/C catalysts, as evidenced in Fig. 24j.

    DFT calculations constructed a predictive model to evaluate the catalytic activity based on directly available parameters such as the curvature of the catalyst surface [213-216]. For example, Fan et al. [215] conducted a theoretical investigation of cobalt-doped nitrogen carbon nanotubes (Co-N-CNTs) catalyst. As illustrated in Fig. 25a, systematic evaluation of single-walled nanotubes with varying chiral indices [SWNT(m,4) where m = 4, 6, 8, 10, 12, 14, 24] demonstrated that strain energy diminishes progressively as the m value rises, eventually approaching negligible levels. This correlation indicates that larger nanotube diameters correspond to reduced internal strain and tension, with atomic interactions approaching those observed in planar graphene structures. Concurrently, both the hydroxyl adsorption free energy (ΔG*OH) and ORR overpotentials (ηORR) exhibited proportional increases with expanding Co-N-CNT diameters (Figs. 25b and c). The computational data reveals that smaller-diameter nanotubes feature Co d-band centers positioned farther from the Fermi level, leading to intensified binding interactions between catalytic sites and reaction intermediates. The strong interaction between reaction intermediates and catalytic surfaces impedes the detachment of water molecules produced during the final reaction phase. As nanotube dimensions expand, the d-band center position of cobalt atoms shifts toward the Fermi energy level, subsequently weakening the interaction intensity between catalytic intermediates and active sites. Various Co-N-CNT configurations spanning diameters from (14,4) to (24,4) demonstrate exceptionally low ηORR between 0.23V and 0.27 V. Research by Zhang's team [216] revealed that displaced Sn atoms form distinctive SnN4 pyramidal structures. Fig. 25d illustrates how these protruding tin atoms generate geometric strain variations across different carbon substrates before oxygen intermediate adsorption, creating contrasting adsorption behavior patterns between curved Sn-N-CNT surfaces and planar Sn-N-GQD systems. The structural distortion caused by *OH and *OOH attached to Sn atoms within Sn-N-CNTs disrupted the linear correlation governing oxygen intermediate adsorption energies (Fig. 25e). Consequently, Sn-N-(20,0) and (25,0) CNT configurations demonstrated remarkable ORR efficiency, exhibiting minimal overpotentials of 0.28 V as evidenced by electrochemical measurements (Fig. 25f).

    Figure 25

    Figure 25.  DFT prediction of strain in M-N-C. (a) The strain energy change with increasing m of Co-N-CNTs. (b) EOH as a linear relationship between the d-band center of Co atom in Co-N-CNTs. (c) ΔG*OH as a function of m of Co-N-CNTs. Reproduced with permission [215]. Copyright 2023, Elsevier. (d) Height (hSn) and the apex angle (θ) of the Sn-N4 square pyramid (depicted in the inset) of Sn-N-CNTs and Sn-N-GQDs. Tensile strain εSn applied to the Sn-N4 pyramid of Sn-N4-CNTs and the compressive strain εSn applied to the Sn-N4 pyramid of Sn-N4-GQDs (taken Sn-N4 of Sn-N4-Gra as the equilibrium state), as schematically illustrated in the inset. (e) ΔG*OOH-ΔG*O versus ΔG*OH on Sn-N-CNTs. (f) Volcano plot relationship between ΔG*OH and the calculated overpotential of ORR. Reproduced with permission [216]. Copyright 2023, American Chemical Society.

    Transition metal nitride (TMN) based materials have been widely facilitated as non-precious metal catalysts for ORR in alkaline media (Figs. 26a and b) [217]. Abruña et al. [218] showed how a well-defined TMN governs/controls the formed oxide surface and the resulting ORR electrocatalytic activity. The atomic-level structure models of the Mn3O4 shell and the MnN core were visualized by using HAADF-STEM images, and the interfacial relationship between them was revealed (Figs. 26c and d). The lattice mismatch between Mn3O4 and MnN results in strain in the growth of Mn3O4 layer. Expansion strain was experimentally observed from the core to the shell region, indicating a tensile strain in the Mn3O4 layer along the [010] direction (Fig. 26e). DFT calculations revealed that compressive strain leads to destabilization of *OH binding, the *OH removal is made easier (the binding energy of *OH is -2.32 eV) on the 5% compressed Mn3O4 (001) surface and more difficult (the binding energy of *OH is -2.83 eV) on the 5% expanded Mn3O4 (001) surface. Such the expansively strained Mn3O4 surface could strengthen the *OH binding and result in a more hydroxylated surface, which increasing the intrinsic activity of ORR. The MA of catalyst is 266 A/g and E1/2 is 0.870 V vs. RHE. And it also displayed impressive ORR stability under ADT with an E1/2 decay of 8 mV after 10,000 potential cycles.

    Figure 26

    Figure 26.  Strain in transition metal nitride/oxide. (a) Schematic synthesis procedure of metal nitrides (MxN) supported on high-surface area carbon via nitridation with ammonia. (b) Comparison of the MA of all MxN/C measured at 0.85 V vs. RHE. Reproduced with permission [217]. Copyright 2022,Wiley-VCH. (c) Schematic atomic model of Mn3O4 shell and MnN core structure along MnN [100] and MnN [110]. (d) Atomic-resolution image of MnN along the [110] projection and Mn3O4 along the [100] projection. (e) In-plane strain measurements from the atom layers in (d). Reproduced with permission [218]. Copyright 2024, Nature. (f) Structural transformation of MMO spinel catalyst Reproduced with permission [219]. Copyright 2022, Wiley-VCH. (g) Computed nanoparticle strain variations versus electrochemical potential. (h) Cyclic voltammetry current profile (green) with corresponding strain responses during cathodic (red) and anodic (blue) potential sweeps. (i) Mechanical model visualization depicting adsorbate-induced surface stress in nanoparticle analogs to pressurized thin-walled containers. (j) CV current trace spanning 0.05-1.4 V (green) with concurrent strain measurements. Reproduced with permission [221]. Copyright 2025, Nature.

    Transition metal oxide [219] (TMO) is promising next-generation electrocatalyst (Fig. 26f) that show comparable ORR reactivity to that of Pt in alkaline fuel cells. However, the specific mechanism of how the structure and morphology of nanoparticles affect the ORR activity and the stability of nanoparticles is still unclear [220]. Singer et al. [221] analyzed the strain changes of Co-Mn oxides during CV process in different potential ranges by in-situ XRD, indicating that. They exhibit good structural stability and reversibility under fuel cell operating conditions. Theoretical calculations show that oxygen vacancy or intercalation is the main source of strain, and the reduction of Mn is the driving force of tetragonal phase formation, which provides basic understanding of the catalytic performance of Co-Mn spinel under extreme conditions. The results showed that the strain varied with the applied potential and showed different behavior in different potential range. As CV from 0.2 V to 1.4 V, the strain shows hysteresis behavior, and the local maximum and minimum points occur when the current crosses zero, indicating that the direction of strain evolution changes with the current direction. The maximum strain was ~0.1% in the CV of 0.05 V to 1.4 V, and the strain remained almost constant during negative potential scanning. The strain behavior under both CV conditions is reversible, indicating that the material shows improving structural stability and reversibility under normal fuel cell operating conditions. However, the strain behavior at low potentials (0.05 V) differed from that at higher potentials (0.2 V), at 0.05 V vs. RHE, XRD observed a phase transition from cubic to tetragonal, which was accompanied by a 2.5% contraction in interlayer spacing. Moreover, as the potential rebounds to 2 V, the tetragonal phase partially recovers to the cubic phase, indicating that this phase transition has a certain degree of reversibility. It is indicating that the structural response of the material at extremely low potentials was different from that under normal operating conditions (Figs. 26g-j). The Co-Mn oxides catalyst exhibited a E1/2 of 0.89 V in 1 mol/L KOH, equal to the benchmark activity of Pt/C. As for the stability, the Co-Mn oxides catalyst turns out to be more stable than Pt under the test protocol of potential cycling. The power density of the cell employing the Co-Mn oxides reaches 1.1 W/cm2 at 2.5 A/cm2 at 60 ℃ [222,223].

    The strain generated by the core-shell structure can effectively improve the ORR activity of TMO [224,225]. Robinson et al. [225] developed a core-shell spinel oxide nanocrystal with tunable shell thickness through colloidal synthesis methods, which is composed of a nickel-doped iron spinel oxide (NFO) core and a cobalt-manganese spinel oxide (CMO) shell. They controlled the shell thickness while maintaining the same shell composition and particle dispersity, allowing for a systematic comparison of shell thickness and ORR activity by modifying the synthesis parameters. It was found that the b and c lattice parameters increase slightly from shell growth of 1 to 3 shells, while the lattice constant remains mostly flat, and then at the 5 shells overgrowth, both the b and c lattice directions show a large expansion, while the lattice experiences a small contraction using the orthorhombic lattice fitting. The value of 0.893 V for the 1-shell sample was within 11 mV of the Pt/C reference material (Fig. 27a). The clear decrease in ORR activity with increasing shell size (Figs. 27b and c) suggests that thicker shells produce larger tensile strains, resulting in lower ORR activity. Notably, the decline in activity with shell thickness is rapid, with a significant decrease observed after just 5 monolayers. While the spinel oxides compare somewhat less favorably to Pt/C in most metrics, when cost is considered, the spinel outperform the Pt/C by over 600-fold.

    Figure 27

    Figure 27.  Strain in spinel/perovskite catalysts. (a) Half-wave potential for 1 to 5 CMO shell samples, CMO and Pt/C. (b) Half-wave potential vs. lattice constant and (c) mass activity vs. lattice constant for 1 to 5 CMO shell samples. Reproduced with permission [225]. Copyright 2025, American Chemical Society. (d) Structural representations of PBSCF-c and BSCFW-c crystalline phases. (e) Temperature-dependent lattice mismatch evolution between PBSCF-c and BSCFW-c polymorphs. (f) Electrochemical impedance spectra (normalized by active surface area) for symmetrical half-cells employing BSPCFW electrodes. (g) Comparative polarization resistance (Rp) values for PBSCF, PBSCF-s, and BSPCFW cathodes under varying thermal conditions. (h) Long-term Rp stability assessment of symmetrical cells with PBSCF and BSPCFW electrodes at 650 ℃ operational temperature. Reproduced with permission [228]. Copyright 2024, Wiley-VCH.

    In addition, lattice tensile stresses were introduced in situ using lattice mismatch strains of perovskite composites containing transition metal oxides. It can enhance the ion-electron transport characteristics of perovskite composite cathode materials, thereby accelerating the electrode reaction kinetics, improving the ORR catalytic activity of cathode materials at low temperatures, and enhancing the long-term stability of the materials [226-228]. Zhao et al. [228] designed (Ba0.5Sr0.5)0.75Pr0.25Co0.575Fe0.3W0.125O3-δ (BSPCFW) perovskite composite cathode based on two perovskite materials with different unit cell parameters, PrBa0.5Sr0.5Co1.5Fe0.5O5+δ (PBSCF-s) (3.85 Å) and BaSrCoFe0.25W0.75O6-δ (BSCFW) (8.00 Å). BSPCFW in situ self-assembly to form two cubic perovskite structure materials, that is, simple perovskite (SP) Pr0.38 Ba0.25Sr0.37Co0.62Fe0.38O3-δ (PBSCF-c) and double perovskite (DP) Ba1.30Sr0.70Co1.0Fe0.25W0.75O6-δ (BSCFW-c). The two phases of PBSCF-c and BSCFF-c form a nanocomposite structure, and the interfaces of the two phases are coherent. There is a 3% lattice mismatch strain between PBSCF-c and BSCFF-c, thereby introducing beneficial lattice tensile stress into the PBSCF-c phase. As shown in Fig. 27d, the PBSCF-c phase in the composite perovskite exhibits a lattice tensile strain of 0.52%. As depicted in Fig. 27e, although the lattice mismatch strain between the SP and DP phases decreases with increasing the temperature, it remains above 2% below 1000 ℃. The lattice parameter of the SP phase can reach equilibrium within a very short time of 600 s at the low temperature of 550 ℃, indicating a very fast ORR kinetics at low temperatures. The polarization resistances (Rp) are only 0.007, 0.012, 0.017, 0.034, and 0.068 Ω cm2 at 800, 750, 700, 650, and 600 ℃, respectively. Even lowering the temperature down to 550 ℃, the Rp is still just 0.190 Ω cm2 (Fig. 27f). As shown in Fig. 27g, the Rp of the BSPCFW composite cathode still presents a 30% lower than that of the pure PBSCF-s perovskite, while the weight content of the active phase PBSCF-c in the composite is 68 wt%. BSPCFW exhibits a lower polarization resistance, indicating that lattice tensile stress significantly enhances the ORR reactivity of the composite cathode. The electrode reaction kinetics process solution indicates that lattice tensile stress promotes the charge transfer and ion migration processes in the cathode ORR reaction, and the composite cathode exhibits excellent low-temperature catalytic activity. The BSPCFW cathode also showed excellent storage resistance and long-term service stability, the material polarization resistance remained stable after 1280 h of operation at 650 ℃ (Fig. 27h).

    Strain engineering has emerged as a pivotal strategy in catalyst design, owing to its substantial influence on atomic sequence and lattice structure, and it is garnering increasing attention from the scientific community. This review delineates six distinct types of strain arising from various origin, providing a comprehensive framework for understanding the role that strain plays in ORR catalytic performance enhancement. Despite the promising potential of strain engineering to enhance catalytic performance, several challenges remain in its application.

    Existing synthesis methods (e.g., alloying, core-shell preparation) cannot achieve atomic-level precise control of strain, especially for large-scale synthesis. The other primary issue impeding precise strain management is the absence of universal, controllable, and interface-independent methods for dynamic adjustment. While the intrinsic strain of two-dimensional nanosheets can be modulated through atomic layer thickness, the technical barriers associated with atomic-level precision in synthesis, such as achieving uniformity in chemical vapor deposition thickness, impede large-scale applications. Thus, future research should concentrate on overcoming the limitations inherent in traditional interface-dependent stress regulation, developing dynamic strain-engineering methods that can universally adapt to various material systems in response to the reaction environment. Additionally, the integration of machine learning into the design process could facilitate the construction of a “composition-synthesis parameters-lattice strain” deep learning model, allowing for the precise prediction of strain values based on established stress-response principles. Moreover, innovative techniques for constructing localized stress fields should be explored.

    Conversely, the enhancement of catalytic activity through stress often compromises structural durability, a challenge stemming from the complex interplay between stress, defects, and structural integrity. For instance, in noble metal systems, while stress can optimize the adsorption energy of hydroxyl group (*OH), which enhances ORR activity, the relaxation of stress during cycling may lead to surface atomic reconstruction or lattice distortion, consequently reducing the density of active sites. Moreover, to introduce high strain, ultra-thin shells or highly defective structures are often used. However, such structures tend to collapse during reactions, leading to active site loss. To address these challenges of trade-offs between strain-induced activity enhancement and long-term stability, the establishment of a multiple scale kinetic model is essential for quantitatively predicting the performance degradation trajectory of catalysts over their operational lifespan. At the material design level, adaptive stress-relief structures can be introduced, such as creating sub-nanometer pore channels at grain boundaries, facilitating local strain relief without compromising overall structural integrity. Simultaneously, a composite system combining rigid frameworks with flexible active sites can be developed, which help maintain a high retention rate of compressive strain over multiple cycles, thereby achieving a synergistic enhancement of both activity and durability.

    Current characterization techniques are insufficient for accurately quantifying and decoupling the myriad parameters of strain at the microscale. Existing methods, such as X-ray diffraction and X-ray photoelectron spectroscopy, can only indirectly infer the strain type through lattice expansion or metal ion satellite peak intensities. These limitations hinder the establishment of spatial correlations between stress distribution and active sites, thereby impeding precise analyses of structure-activity relationships. Thus, the development of coupled in-situ systems is imperative. A key approach involves integrating synchrotron X-ray nano-tomography with high-resolution electron backscatter diffraction technology to track the evolution of stress fields within individual particles in real time during the ORR process. Additionally, the development of spectroscopic-mechanical coupling probes, such as a combined surface-enhanced Raman spectroscopy (SERS) and atomic force microscopy (AFM) device, would allow simultaneous monitoring of the adsorption configurations of intermediates and surface deformations under stress, establishing a direct correlation between changes in adsorption energy and localized strain. Moreover, integrating density functional theory, molecular dynamics simulations with experiments observations enables quantify individual contributions from strain to other ingredients, guiding the design of targeted catalysts.

    Strain engineering extends beyond the ORR, presenting transformative potential for various energy-related processes, such as carbon dioxide reduction and water splitting. By integrating strain effects with complementary strategies, next-generation catalysts could achieve unprecedented levels of efficiency, stability, and cost-effectiveness. This advancement is crucial for promoting the commercialization of fuel cells and metal-air batteries.

    Yuan Zhao: Writing – review & editing. Hanqi Yu: Writing – review & editing. Jiuchao Tang: Supervision. Yingmei Li: Writing – review & editing. Xue Yong: Writing – review & editing, Supervision. Xin Tu: Supervision. Jing Wang: Supervision, Conceptualization.

    The authors declare that they have no known competing 7inancial interests or personal relationships that could have appeared to in7luence the work reported in this paper.

    The authors thank the financial supports from the Hebei Science Foundation (Nos. B2025203032, B2025203050), Hebei provincial Department of Science and Technology (No. 226Z4404G).


    1. [1]

      Z. Liang, D. Shen, Y. Wei, et al., Adv. Mater. 36 (2024) 2408634. doi: 10.1002/adma.202408634

    2. [2]

      R.Z. Snitkoff-Sol, O. Rimon, A.M. Bond, et al., Nat. Catal. 7 (2024) 139–147. doi: 10.1038/s41929-023-01086-0

    3. [3]

      D. Shen, F. Sun, Z. Liang, et al., Angew. Chem. Int. Ed. 64 (2025) e202505937. doi: 10.1002/anie.202505937

    4. [4]

      T. Chen, X.K. Zhang, H.C. Wang, et al., Nat. Commun. 16 (2025) 3308. doi: 10.1038/s41467-025-58679-5

    5. [5]

      C.Q. Zhang, P.Y. Shan, Y.Y. Zou, et al., Nat. Sustain. 8 (2025) 542–552. doi: 10.1038/s41893-025-01538-4

    6. [6]

      H.X. Xu, D.J. Cheng, D.P. Cao, et al., Nat. Catal. 7 (2024) 207–218. doi: 10.1038/s41929-023-01106-z

    7. [7]

      J. Li, S. Zou, J. Huang, et al., Chin. Chem. Lett. 34 (2023) 107222. doi: 10.1016/j.cclet.2022.02.027

    8. [8]

      J. Jiang, M. Tong, D. Shen, et al., Adv. Funct. Mater. 35 (2025) 2500065. doi: 10.1002/adfm.202500065

    9. [9]

      H. Jin, S. Zou, Q. Wen, et al., Chin. Chem. Lett. 34 (2023) 107441. doi: 10.1016/j.cclet.2022.04.039

    10. [10]

      Y.X. Mo, L.L. Liao, D.Y. Li, et al., Chin. Chem. Lett. 34 (2023) 107130. doi: 10.1016/j.cclet.2022.01.023

    11. [11]

      W. Liu, C. Zhang, J. Zhang, et al., Appl. Catal. B: Environ. 310 (2022) 121312. doi: 10.1016/j.apcatb.2022.121312

    12. [12]

      L.S. Peng, J. Yang, Y.Q. Yang, et al., Adv. Mater. 34 (2022) 2202544. doi: 10.1002/adma.202202544

    13. [13]

      Q. Liu, P. Qiao, D. Shen, et al., Energy Environ. Sci. 18 (2025) 2839–2851. doi: 10.1039/d4ee05508j

    14. [14]

      S. Akula, M. Mooste, J. Kozlova, et al., Chem. Eng. J. 458 (2023) 141468. doi: 10.1016/j.cej.2023.141468

    15. [15]

      S.D. Bhoyate, J. Kim, F.M. de Souza, et al., Coord. Chem. Rev. 474 (2023) 214854. doi: 10.1016/j.ccr.2022.214854

    16. [16]

      Y.J. Li, Y.J. Ding, B. Zhang, et al., Energy Environ. Sci. 16 (2023) 2629–2636. doi: 10.1039/d3ee00747b

    17. [17]

      Z.C. Nie, M.S. Chen, L. Zhang, et al., Chem. Eng. J. 463 (2023) 142411. doi: 10.1016/j.cej.2023.142411

    18. [18]

      X. Qin, P.K. Cao, X. Quan, et al., Environ. Sci. Technol. 57 (2023) 2907–2917. doi: 10.1021/acs.est.2c06981

    19. [19]

      W.J. Shao, R. Yan, M. Zhou, et al., Electrochem. Energy Rev. 6 (2023) 11. doi: 10.1007/s41918-023-00181-x

    20. [20]

      C. Zhang, W.Q. Shen, K. Guo, et al., J. Am. Chem. Soc. 145 (2023) 11589–11598. doi: 10.1021/jacs.3c00689

    21. [21]

      G. Xing, M. Tong, P. Yu, et al., Angew. Chem. Int. Ed. 61 (2022) e202211098. doi: 10.1002/anie.202211098

    22. [22]

      X. Wang, X. Zhang, M. Jiao, et al., Chin. J. Catal. 77 (2025) 227–235. doi: 10.1016/S1872-2067(25)64768-1

    23. [23]

      H. Wang, L. Cao, Y. Feng, et al., Chin. Chem. Lett. 34 (2023) 107601. doi: 10.1016/j.cclet.2022.06.024

    24. [24]

      J.H.K. Pfisterer, Y. Liang, O. Schneider, et al., Nature 549 (2017) 74–77. doi: 10.1038/nature23661

    25. [25]

      Y. Jia, L. Zhang, L. Zhuang, et al., Nat. Catal. 2 (2019) 688–695. doi: 10.1038/s41929-019-0297-4

    26. [26]

      C. Xie, Z. Niu, D. Kim, et al., Chem. Rev. 120 (2020) 1184–1249. doi: 10.1021/acs.chemrev.9b00220

    27. [27]

      J.S. Bates, Nat. Chem. 17 (2024) 318–324. doi: 10.1038/s41557-024-01731-6

    28. [28]

      S. Xie, H. Jin, C. Wang, et al., Chin. Chem. Lett. 34 (2023) 107681. doi: 10.1016/j.cclet.2022.07.024

    29. [29]

      H. Li, B. Cai, Y. Song, et al., Chin. Chem. Lett. 34 (2023) 107811. doi: 10.1016/j.cclet.2022.107811

    30. [30]

      J. Huang, L. Sementa, Z. Liu, et al., Nat. Catal. 5 (2022) 513–523. doi: 10.1038/s41929-022-00797-0

    31. [31]

      F. Shi, P. Tieu, H. Hu, et al., Nat. Commun. 15 (2024) 5084. doi: 10.1038/s41467-024-49434-3

    32. [32]

      I. Jang, S. Lee, D.G. Kim, et al., Adv. Mater. 36 (2024) 2403273. doi: 10.1002/adma.202403273

    33. [33]

      G. Bae, M.M. Kim, M.H. Han, et al., Nat. Catal. 6 (2023) 1140–1150. doi: 10.1038/s41929-023-01039-7

    34. [34]

      X. Wu, G. Liu, S. Yang, et al., Chin. Chem. Lett. 34 (2023) 107540. doi: 10.1016/j.cclet.2022.05.054

    35. [35]

      T. He, W. Wang, F. Shi, et al., Nature 598 (2021) 76–81. doi: 10.1038/s41586-021-03870-z

    36. [36]

      A. Khorshidi, J. Violet, J. Hashemi, et al., Nat. Catal. 1 (2018) 263–268. doi: 10.1038/s41929-018-0054-0

    37. [37]

      X. Xu, T. Liang, D. Kong, et al., Mater. Today Nano 14 (2021) 100111. doi: 10.1016/j.mtnano.2021.100111

    38. [38]

      T.Nilsson Pingel, M. Jørgensen, A.B. Yankovich, et al., Nat. Commun. 9 (2018) 2722. doi: 10.1038/s41467-018-05055-1

    39. [39]

      Q. Feng, S. Zhao, D. He, et al., J. Am. Chem. Soc. 140 (2018) 2773–2776. doi: 10.1021/jacs.7b13612

    40. [40]

      M. Wang, Q. Sun, Z. Fan, et al., J. Mater. Chem. A 11 (2023) 4037–4044. doi: 10.1039/d2ta08454f

    41. [41]

      S. Zuo, Z.P. Wu, D. Xu, et al., Nat. Commun. 15 (2024) 9514. doi: 10.1038/s41467-024-53763-8

    42. [42]

      Y. Du, F. Xie, M. Lu, et al., Nat. Commun. 15 (2024) 1780. doi: 10.1038/s41467-024-46216-9

    43. [43]

      C. Atlan, C. Chatelier, I. Martens, et al., Nat. Mater. 22 (2023) 754–761. doi: 10.1038/s41563-023-01528-x

    44. [44]

      Y.H. Wang, L. Li, J.H. Shi, et al., Adv. Sci. 10 (2023) 2303321. doi: 10.1002/advs.202303321

    45. [45]

      K.C. Qian, Y. Yan, S.B. Xi, et al., Small 17 (2021) 2102970. doi: 10.1002/smll.202102970

    46. [46]

      L. Wang, Z. Zeng, W. Gao, et al., Science 363 (2019) 870–874. doi: 10.1126/science.aat8051

    47. [47]

      M. Li, Z. Zhao, T. Cheng, et al., Science 354 (2016) 1414–1419. doi: 10.1126/science.aaf9050

    48. [48]

      G. Liu, A.J. Shih, H. Deng, et al., Nature 626 (2024) 1005–1010. doi: 10.1038/s41586-024-07090-z

    49. [49]

      J.K. Nørskov, J. Rossmeisl, A. Logadottir, et al., J. Phys. Chem. B 108 (2004) 17886–17892. doi: 10.1021/jp047349j

    50. [50]

      M. Luo, S. Guo, Nat. Rev. Mater. 2 (2017) 17059. doi: 10.1038/natrevmats.2017.59

    51. [51]

      J.R. Kitchin, J.K. Nørskov, M.A. Barteau, et al., Phys. Rev. Lett. 93 (2004) 156801. doi: 10.1103/PhysRevLett.93.156801

    52. [52]

      Z. Wang, S. Chen, W. Wu, et al., Adv. Mater. 35 (2023) 2301310. doi: 10.1002/adma.202301310

    53. [53]

      L. Bu, N. Zhang, S. Guo, et al., Science 354 (2016) 1410–1414. doi: 10.1126/science.aah6133

    54. [54]

      X. Zhao, C. Xi, R. Zhang, et al., ACS Catal. 10 (2020) 10637–10645. doi: 10.1021/acscatal.0c03036

    55. [55]

      N. He, S. Wu, W. Yu, et al., Sci. China Mater. 68 (2025) 180–188. doi: 10.1007/s40843-024-3166-2

    56. [56]

      R.P. Jansonius, L.M. Reid, C.N. Virca, et al., ACS Energy Lett. 4 (2019) 980–986. doi: 10.1021/acsenergylett.9b00191

    57. [57]

      R. Cepitis, N. Kongi, J. Rossmeisl, et al., ACS Energy Lett. 8 (2023) 1330–1335. doi: 10.1021/acsenergylett.3c00068

    58. [58]

      A. Bao, Y.H. Gu, Y.X. Zhang, et al., Carbon Energy 6 (2024) e519. doi: 10.1002/cey2.519

    59. [59]

      C. Lim, A.R. Fairhurst, B.J. Ransom, et al., ACS Catal. 13 (2023) 14874–14893. doi: 10.1021/acscatal.3c03321

    60. [60]

      M.S. Ozóorio, J. Rossmeisl, ACS Catal. 16 (2026) 17075–17089. doi: 10.1021/acscatal.6c04024

    61. [61]

      Y. Zhuang, J. Yang, L. Meng, et al., Ind. Chem. Mater. 1 (2023) 458–464. doi: 10.1039/d3im00056g

    62. [62]

      L.Z. Yang, Q.L. Liu, R. Han, et al., Appl. Catal. B: Environ. 309 (2022) 121224. doi: 10.1016/j.apcatb.2022.121224

    63. [63]

      X.L. Tian, X. Zhao, Y.Q. Su, et al., Science 366 (2019) 850–856. doi: 10.1126/science.aaw7493

    64. [64]

      F. Xiao, Q. Wang, G.L. Xu, et al., Nat. Catal. 5 (2022) 503–512. doi: 10.1038/s41929-022-00796-1

    65. [65]

      X.X. Zhu, L. Huang, M. Wei, et al., Appl. Catal. B: Environ. 281 (2021) 119460. doi: 10.1016/j.apcatb.2020.119460

    66. [66]

      Y. Nie, Y. Sun, B. Song, et al., Angew. Chem. Int. Ed. 63 (2024) e202317987. doi: 10.1002/anie.202317987

    67. [67]

      F. Lin, M. Li, L. Zeng, et al., Chem. Rev. 123 (2023) 12507–12593. doi: 10.1021/acs.chemrev.3c00382

    68. [68]

      M. Song, G. Luo, Q. Zhang, et al., Sci. China Chem. 68 (2024) 536–542. doi: 10.1080/24694452.2023.2285371

    69. [69]

      H. Zhu, S. Sun, J. Hao, et al., Energy Environ. Sci. 16 (2023) 619–628. doi: 10.1039/d2ee03185j

    70. [70]

      S. Jiang, Y. Yu, H. He, et al., Small 20 (2024) 2310786. doi: 10.1002/smll.202310786

    71. [71]

      X. Zou, J. Xie, Z. Mei, et al., Proc. Natl. Acad. Sci. U. S. A. 121 (2024) e2313239121. doi: 10.1073/pnas.2313239121

    72. [72]

      J.S. Liang, Y.Y. Wan, H.F. Lv, et al., Nat. Mater. 23 (2024) 1259–1267. doi: 10.1038/s41563-024-01901-4

    73. [73]

      R.Y. Shao, X. Niu, X.C. Xu, et al., Nano Lett. 24 (2024) 5578–5584. doi: 10.1021/acs.nanolett.4c00898

    74. [74]

      J.W. Lankman, M.P. Perich, X. Liu, et al., ACS Catal. 16 (2026) 14531–14544. doi: 10.1021/acscatal.6c02868

    75. [75]

      L.X. Luo, C.H. Fu, Y.G. Guo, et al., ACS Nano 17 (2023) 2992–3006. doi: 10.1021/acsnano.2c11627

    76. [76]

      Y.P. Zhang, H.H. Wei, Z.Q. Wang, et al., J. Phys. Chem. C 128 (2024) 15476–15486. doi: 10.1021/acs.jpcc.4c04875

    77. [77]

      J. Guan, S. Yang, T. Liu, et al., Angew. Chem. Int. Ed. 60 (2021) 21899–21904. doi: 10.1002/anie.202107437

    78. [78]

      D. Liu, Q. Zeng, C. Hu, et al., ACS Catal. 12 (2022) 9092–9100. doi: 10.1021/acscatal.2c02274

    79. [79]

      S. Zhu, Y. Liu, Y. Gong, et al., Small 20 (2024) 2305062. doi: 10.1002/smll.202305062

    80. [80]

      M. Liu, S. Li, Y. Fang, et al., Langmuir 36 (2020) 7427–7438. doi: 10.1021/acs.langmuir.0c00971

    81. [81]

      Z. Yu, H. Deng, Q. Yao, et al., Nat. Commun. 15 (2024) 9346. doi: 10.1038/s41467-024-53607-5

    82. [82]

      H. Jin, Z.W. Xu, Z.Y. Hu, et al., Nat. Commun. 14 (2023) 1518. doi: 10.1038/s41467-023-37268-4

    83. [83]

      J. Zhu, A.O. Elnabawy, Z. Lyu, et al., Mater. Today 35 (2020) 69–77. doi: 10.1016/j.mattod.2019.11.002

    84. [84]

      H. Wang, X.K. Gu, X. Zheng, et al., Sci. Adv. 5 (2019) eaat6413. doi: 10.1126/sciadv.aat6413

    85. [85]

      S. Chen, D.M. Huang, D.Y. Liu, et al., Appl. Catal. B: Environ. 291 (2021) 120065. doi: 10.1016/j.apcatb.2021.120065

    86. [86]

      X. Zhao, J.B. Chen, Z.H. Bi, et al., Adv. Sci. 10 (2023) 2205889. doi: 10.1002/advs.202205889

    87. [87]

      M. Xie, Z. Lyu, R. Chen, et al., J. Am. Chem. Soc. 143 (2021) 8509–8518. doi: 10.1021/jacs.1c04160

    88. [88]

      C. Wang, H. Daimon, T. Onodera, et al., Angew. Chem. Int. Ed. 47 (2008) 3588–3591. doi: 10.1002/anie.200800073

    89. [89]

      F. He, Y.J. Liu, Q.H. Cai, et al., New J. Chem. 44 (2020) 16135–16143. doi: 10.1039/d0nj03645e

    90. [90]

      C. Chen, Y.J. Kang, Z.Y. Huo, et al., Science 343 (2014) 1339–1343. doi: 10.1126/science.1249061

    91. [91]

      J.C. Guo, L. Gao, X. Tan, et al., Angew. Chem. Int. Ed. 60 (2021) 10942–10949. doi: 10.1002/anie.202100307

    92. [92]

      H. Yoon, H.J. Song, B. Ju, et al., ACS Sustain. Chem. Eng. 10 (2022) 15319–15327. doi: 10.1021/acssuschemeng.2c05246

    93. [93]

      M. Liu, S. Zhou, M. Figueras-Valls, et al., Adv. Energy Mater. 34 (2024) 2404677. doi: 10.1002/adfm.202404677

    94. [94]

      S. Ding, B. Xia, M. Li, et al., Energy Environ. Sci. 16 (2023) 3363–3372. doi: 10.1039/d3ee00509g

    95. [95]

      N. Li, M.Y. Li, K. Guo, et al., Adv. Energy Mater. 14 (2024) 2401008. doi: 10.1002/aenm.202401008

    96. [96]

      K. Guo, Z.M. He, S. Lu, et al., Adv. Funct. Mater. 33 (2023) 2302100. doi: 10.1002/adfm.202302100

    97. [97]

      S. Ji, Y. Wang, H. Liu, et al., Adv. Energy Mater. 34 (2024) 2314621. doi: 10.1002/aenm.202314621

    98. [98]

      P. Santra, S. Ghaderzadeh, M. Ghorbani-Asl, et al., npj 2D Mater. Appl. 8 (2024) 33. doi: 10.1038/s41699-024-00472-x

    99. [99]

      Y.Y. Ha, J.L. Oberst, Z.H. Zeng, et al., Electrochim. Acta 260 (2018) 400–406. doi: 10.1016/j.electacta.2017.12.039

    100. [100]

      K. Wang, Y. Hu, X. Liu, et al., Nat. Commun. 16 (2025) 2094. doi: 10.1038/s41467-025-57140-x

    101. [101]

      S. Ye, W. Chen, Z. Ou, et al., Angew. Chem. Int. Ed. 64 (2025) e202414989. doi: 10.1002/anie.202414989

    102. [102]

      A.E. Thorarinsdottir, D.P. Erdosy, C. Costentin, et al., Nat. Catal. 6 (2023) 425–434. doi: 10.1038/s41929-023-00958-9

    103. [103]

      L. Yan, B.B. Xie, C. Yang, et al., Adv. Energy Mater. 13 (2023) 2204245. doi: 10.1002/aenm.202204245

    104. [104]

      Y.T. Yan, J.H. Lin, K.K. Huang, et al., J. Am. Chem. Soc. 145 (2023) 24218–24229. doi: 10.1021/jacs.3c08598

    105. [105]

      X. Zhang, K. Zhao, Z.H. Gu, Acc. Chem. Res. 55 (2022) 1620–1633. doi: 10.1021/acs.accounts.2c00175

    106. [106]

      C. Vogt, B.M. Weckhuysen, Nat. Rev. Chem. 6 (2022) 89–111. doi: 10.1038/s41570-021-00340-y

    107. [107]

      S. Saini, J. Halldin Stenlid, F. Abild-Pedersen, npj Comput. Mater. 8 (2022) 163. doi: 10.1038/s41524-022-00846-z

    108. [108]

      Y. Meng, Y.M. Zhao, J.C. Li, et al., npj Asia Mater. 15 (2023) 14. doi: 10.1038/s41427-022-00441-0

    109. [109]

      P. Rao, D. Wu, T.J. Wang, et al., eScience 2 (2022) 399–404. doi: 10.1016/j.esci.2022.05.004

    110. [110]

      G. Chen, R. Lu, C. Li, et al., Adv. Mater. 35 (2023) 2300907. doi: 10.1002/adma.202300907

    111. [111]

      H. Li, W. Wang, S. Xue, et al., J. Am. Chem. Soc. 146 (2024) 9124–9133. doi: 10.1021/jacs.3c14354

    112. [112]

      J. Su, C.B. Musgrave, Y. Song, et al., Nat. Catal. 6 (2023) 818–828. doi: 10.1038/s41929-023-01005-3

    113. [113]

      C.B. Musgrave Ⅲ, J. Su, P. Xiong, et al., J. Am. Chem. Soc. 147 (2025) 3786–3795. doi: 10.1021/jacs.4c16637

    114. [114]

      J. Zhang, Y. Mou, W. Suo, et al., Adv. Energy Mater. 35 (2024) 2417621.

    115. [115]

      L. Zhang, S. Jiang, W. Ma, et al., Chin. J. Catal. 43 (2022) 1433–1443. doi: 10.1016/S1872-2067(21)63961-X

    116. [116]

      X. Wang, L. Zhang, N. Wang, et al., Chem. Eng. J. 499 (2024) 156609. doi: 10.1016/j.cej.2024.156609

    117. [117]

      L. Bu, J. Liang, F. Ning, et al., Adv. Mater. 35 (2023) 2208672. doi: 10.1002/adma.202208672

    118. [118]

      L. Huo, M. Lv, M. Li, et al., Adv. Mater. 36 (2024) 2312868. doi: 10.1002/adma.202312868

    119. [119]

      S. Wei, R. Yang, Z. Wang, et al., Adv. Mater. 36 (2024) 2404692. doi: 10.1002/adma.202404692

    120. [120]

      S. Zhou, W. Bi, J. Zhang, et al., Adv. Mater. 36 (2024) 2400808. doi: 10.1002/adma.202400808

    121. [121]

      X. Deng, Z. Jiang, Y. Chen, et al., Chin. Chem. Lett. 34 (2023) 107389. doi: 10.1016/j.cclet.2022.03.112

    122. [122]

      Z.W. Seh, J. Kibsgaard, C.F. Dickens, et al., Science 355 (2017) eaad4998. doi: 10.1126/science.aad4998

    123. [123]

      Z. Jia, Y. Wang, J. Chen, et al., Chin. Chem. Lett. 34 (2023) 107137. doi: 10.1016/j.cclet.2022.01.030

    124. [124]

      A. Ruban, B. Hammer, P. Stoltze, et al., J. Mol. Catal. A: Chem. 115 (1997) 421–429. doi: 10.1016/S1381-1169(96)00348-2

    125. [125]

      M. Mavrikakis, B. Hammer, J.K. Nørskov, Phys. Rev. Lett. 81 (1998) 2819–2822. doi: 10.1103/PhysRevLett.81.2819

    126. [126]

      R.M. Kluge, R.W. Haid, A. Riss, et al., Energy Environ. Sci. 15 (2022) 5181–5191. doi: 10.1039/d2ee01850k

    127. [127]

      X. Li, X. Duan, K. Hua, et al., Carbon Energy 6 (2024) e508. doi: 10.1002/cey2.508

    128. [128]

      X. Li, X. Duan, S. Zhang, et al., Angew. Chem. Int. Ed. 63 (2024) e202400549. doi: 10.1002/anie.202400549

    129. [129]

      W. Zhang, J. Li, Z. Wei, Small 19 (2023) 2300112. doi: 10.1002/smll.202300112

    130. [130]

      X. Yao, Z. Song, X. Yao, et al., Angew. Chem. Int. Ed. 63 (2024) e202318872. doi: 10.1002/anie.202318872

    131. [131]

      G. Cao, S. Yang, J.C. Ren, et al., Nat. Commun. 16 (2025) 1251. doi: 10.1038/s41467-025-56421-9

    132. [132]

      Z. Xu, X. Zhang, X. Wang, et al., ACS Nano 15 (2021) 7131–7138. doi: 10.1021/acsnano.1c00305

    133. [133]

      C. Li, D. Chen, Y.Y. Mao, et al., ACS Catal. 16 (2026) 5703–5712. doi: 10.1021/acscatal.5c08577

    134. [134]

      H. Kuang, Z. Xu, X. Tan, et al., Small 20 (2024) 2308421. doi: 10.1002/smll.202308421

    135. [135]

      L. Zhang, X. Zhang, C. Chen, et al., Angew. Chem. Int. Ed. 63 (2024) e202411123. doi: 10.1002/anie.202411123

    136. [136]

      M. Niu, Q. Guan, W. Yuan, et al., Chem. Eng. J. 503 (2025) 158465. doi: 10.1016/j.cej.2024.158465

    137. [137]

      Z. Huang, Y. Peng, L. Xing, et al., Appl. Catal. B: Environ. 363 (2025) 124775. doi: 10.1016/j.apcatb.2024.124775

    138. [138]

      X. Zou, X. Zhao, B. Pang, et al., Adv. Mater. 36 (2024) 2412954. doi: 10.1002/adma.202412954

    139. [139]

      D. Wang, H.L. Xin, R. Hovden, et al., Nat. Mater. 12 (2013) 81–87. doi: 10.1038/nmat3458

    140. [140]

      T.W. Song, M.X. Chen, P. Yin, et al., Small 18 (2022) 2202916. doi: 10.1002/smll.202202916

    141. [141]

      J.R. Li, S. Sun, Acc. Chem. Res. 52 (2019) 2015–2025. doi: 10.1021/acs.accounts.9b00172

    142. [142]

      J. Guan, J. Zhang, X. Wang, et al., Adv. Mater. 35 (2023) 2207995. doi: 10.1002/adma.202207995

    143. [143]

      R. Gui, H. Cheng, M. Wang, et al., Adv. Mater. 36 (2024) 2307661. doi: 10.1002/adma.202307661

    144. [144]

      M.J. Liu, H.L. Xin, Q. Wu, Phys. Chem. Chem. Phys. 21 (2019) 6477–6484. doi: 10.1039/c8cp06756b

    145. [145]

      J.S. Liang, N. Li, Z.L. Zhao, et al., Angew. Chem. Int. Ed. 58 (2019) 15471–15477. doi: 10.1002/anie.201908824

    146. [146]

      J. Kari, J.P. Olsen, K. Jensen, et al., ACS Catal. 8 (2018) 11966–11972. doi: 10.1021/acscatal.8b03547

    147. [147]

      X. Liu, J. Liang, Q. Li, Chin. J. Catal. 45 (2023) 17–26. doi: 10.1016/S1872-2067(22)64165-2

    148. [148]

      X. Liu, Z.L. Zhao, J.S. Liang, et al., Angew. Chem. Int. Ed. 62 (2023) e202302134. doi: 10.1002/anie.202302134

    149. [149]

      R.Y. Shao, X.C. Xu, Z.H. Zhou, et al., Nat. Commun. 14 (2023) 5896. doi: 10.1038/s41467-023-41590-2

    150. [150]

      L. Zhang, Y. Deng, J. Zhang, et al., Chem. Mater. 36 (2024) 11404–11411. doi: 10.1021/acs.chemmater.4c01968

    151. [151]

      D.Y. Chung, S. Park, H. Lee, et al., ACS Energy Lett. 5 (2020) 2827–2834. doi: 10.1021/acsenergylett.0c01507

    152. [152]

      H. Hojo, M. Gondo, S. Yoshizaki, et al., Nano Lett. 22 (2022) 145–150. doi: 10.1021/acs.nanolett.1c03485

    153. [153]

      H. Ahn, H. Ahn, J. An, et al., Nano Lett. 22 (2022) 9115–9121. doi: 10.1021/acs.nanolett.2c03611

    154. [154]

      A. Mahmood, D. He, S.H. Talib, et al., Adv. Energy Mater. 32 (2022) 2205223.

    155. [155]

      Y. Xiong, Y. Ma, L. Zou, et al., J. Catal. 382 (2020) 247–255. doi: 10.1016/j.jcat.2019.12.025

    156. [156]

      D. Kudo, S. Kaneko, R. Myochi, et al., ACS Appl. Energy Mater. 2 (2019) 4597–4601. doi: 10.1021/acsaem.9b00873

    157. [157]

      J.C. Douglin, J.A. Zamora Zeledón, M.E. Kreider, et al., Nat. Energy 8 (2023) 1262–1272. doi: 10.1038/s41560-023-01385-7

    158. [158]

      G. Wang, J. Guan, L. Xiao, et al., Nano Energy 29 (2016) 268–274. doi: 10.1504/IJETM.2016.10003114

    159. [159]

      W. Jiao, C. Chen, W. You, et al., Appl. Catal. B: Environ. 262 (2020) 118298. doi: 10.1016/j.apcatb.2019.118298

    160. [160]

      W. Jiao, C. Chen, W. You, et al., Adv. Energy Mater. 10 (2020) 1904072. doi: 10.1002/aenm.201904072

    161. [161]

      M. Luo, Z. Zhao, Y. Zhang, et al., Nature 574 (2019) 81–85. doi: 10.1038/s41586-019-1603-7

    162. [162]

      H. Yu, T. Zhou, Z. Wang, et al., Angew. Chem. Int. Ed. 60 (2021) 12027–12031. doi: 10.1002/anie.202101019

    163. [163]

      Y. Chen, M. Sun, M. Wu, et al., ACS Catal. 14 (2024) 9354–9363. doi: 10.1021/acscatal.4c00403

    164. [164]

      H. Fu, H. Huang, Y. Chen, et al., ChemSusChem 17 (2024) e202301221. doi: 10.1002/cssc.202301221

    165. [165]

      J.S. Liang, S.Z. Li, X. Liu, et al., Nat. Catal. 7 (2024) 719–732. doi: 10.1038/s41929-024-01167-8

    166. [166]

      F. Zhang, S. Sun, X. Ge, et al., Chem. Commun. 60 (2024) 3591–3594. doi: 10.1039/d4cc00247d

    167. [167]

      X. Zuo, R. Yan, L. Zhao, et al., J. Mater. Chem. A 10 (2022) 14857–14865. doi: 10.1039/d2ta02597c

    168. [168]

      F. Lin, F. Lv, Q. Zhang, et al., Adv. Mater. 34 (2022) 2202084. doi: 10.1002/adma.202202084

    169. [169]

      L. Chong, J. Wen, J. Kubal, et al., Science 362 (2018) 1276–1281. doi: 10.1126/science.aau0630

    170. [170]

      J. Tian, Y. Song, X. Hao, et al., Adv. Mater. 37 (2025) 2412051. doi: 10.1002/adma.202412051

    171. [171]

      C. Lin, J.L. Li, X. Li, et al., Nat. Catal. 4 (2021) 1012–1023. doi: 10.1038/s41929-021-00703-0

    172. [172]

      H. Su, C.Y. Yang, M.H. Liu, et al., Nat. Commun. 15 (2024) 95. doi: 10.1038/s41467-023-44483-6

    173. [173]

      Y. Qin, T. Yu, S. Deng, et al., Nat. Commun. 13 (2022) 3784. doi: 10.1038/s41467-022-31468-0

    174. [174]

      Y. Qiu, Y.F. Rao, Y.N. Zheng, et al., InfoMat 4 (2022) 3784.

    175. [175]

      L. Li, J. Zhu, F. Kong, et al., Matter 7 (2024) 1517–1532. doi: 10.1016/j.matt.2024.01.019

    176. [176]

      M. Xie, X. Xiao, D. Wu, et al., Nano Res. 17 (2024) 5288–5297. doi: 10.1007/s12274-024-6526-4

    177. [177]

      E.B. Zhu, W. Xue, S.Y. Wang, et al., Nano Res. 13 (2020) 3310–3314. doi: 10.1007/s12274-020-3007-2

    178. [178]

      M.K. Kabiraz, B. Ruqia, J. Kim, et al., ACS Catal. 12 (2022) 3516–3523. doi: 10.1021/acscatal.1c05766

    179. [179]

      T.O. He, W.C. Wang, F.L. Shi, et al., Nature 598 (2021) 76–81.

    180. [180]

      X. Geng, M. Vega-Paredes, Z. Wang, et al., Nat. Commun. 15 (2024) 8534. doi: 10.1038/s41467-024-52919-w

    181. [181]

      H. Yu, G. Zhang, D. Zhang, et al., Adv. Energy Mater. 14 (2024) 2401509. doi: 10.1002/aenm.202401509

    182. [182]

      N. Li, K. Guo, M. Li, et al., J. Am. Chem. Soc. 145 (2023) 24580–24589. doi: 10.1021/jacs.3c09571

    183. [183]

      N. Li, M. Li, K. Guo, et al., Adv. Energy Mater. 14 (2024) 2401008. doi: 10.1002/aenm.202401008

    184. [184]

      L.L. Zhang, P.P. Lu, Y.R. Luo, et al., J. Mater. Chem. A 9 (2021) 9609–9615. doi: 10.1039/d0ta12418d

    185. [185]

      J. Zhang, Y. Chen, M. Tian, et al., Chin. Chem. Lett. 34 (2023) 107886. doi: 10.1016/j.cclet.2022.107886

    186. [186]

      X. Wan, X.F. Liu, Y.C. Li, et al., Nat. Catal. 2 (2019) 259–268. doi: 10.1038/s41929-019-0237-3

    187. [187]

      Y. Ha, B. Fei, X.X. Yan, et al., Adv. Energy Mater. 10 (2020) 2002592. doi: 10.1002/aenm.202002592

    188. [188]

      K. Liu, J.W. Fu, Y.Y. Lin, et al., Nat. Commun. 13 (2022) 2075. doi: 10.1038/s41467-022-29797-1

    189. [189]

      Q.L. Wu, Y. Jia, Q. Liu, et al., Chem 8 (2022) 2715–2733. doi: 10.1016/j.chempr.2022.06.013

    190. [190]

      D.P. Xue, Y.Y. Guo, B.A. Lu, et al., Adv. Sci. 10 (2023) 2302930. doi: 10.1002/advs.202302930

    191. [191]

      X. Feng, G. Chen, Z. Cui, et al., Angew. Chem. Int. Ed. 63 (2024) e202316314. doi: 10.1002/anie.202316314

    192. [192]

      Y. Yu, Y. Wang, F. Yang, et al., Angew. Chem. Int. Ed. 64 (2024) e202415691. doi: 10.1002/anie.202415691

    193. [193]

      F. She, Z. Guo, F. Liu, et al., ACS Catal. 14 (2024) 10928–10938. doi: 10.1021/acscatal.4c01637

    194. [194]

      B. Liu, S. Xu, Y. Gao, et al., J. Am. Chem. Soc. 147 (2025) 4258–4267. doi: 10.1021/jacs.4c14372

    195. [195]

      H.T. Chung, D.A. Cullen, D. Higgins, et al., Science 357 (2017) 479–483. doi: 10.1126/science.aan2255

    196. [196]

      Y.H. He, S.W. Liu, C. Priest, et al., Chem. Soc. Rev. 49 (2020) 3484–3524. doi: 10.1039/c9cs00903e

    197. [197]

      G. Wan, P.F. Yu, H.R. Chen, et al., Small 14 (2018) 1704319. doi: 10.1002/smll.201704319

    198. [198]

      Z. Liang, M. Luo, M. Chen, et al., J. Mater. Chem. A 8 (2020) 20453–20462. doi: 10.1039/d0ta06335e

    199. [199]

      J.Z. Li, M.J. Chen, D.A. Cullen, et al., Nat. Catal. 1 (2018) 935–945. doi: 10.1038/s41929-018-0164-8

    200. [200]

      S.W. Liu, C.Z. Li, M.J. Zachman, et al., Nat. Energy 7 (2022) 652–663. doi: 10.1038/s41560-022-01062-1

    201. [201]

      X.X. Wang, V. Prabhakaran, Y.H. He, et al., Adv. Mater. 31 (2019) 652–663.

    202. [202]

      Y. Sun, J. Wang, Q. Liu, et al., J. Mater. Chem. A 7 (2019) 27175–27185. doi: 10.1039/c9ta08616a

    203. [203]

      H. Chen, J. Wang, Y. Zhao, et al., Mater. Today Energy 45 (2024) 101661. doi: 10.1016/j.mtener.2024.101661

    204. [204]

      J. Chen, J. Wang, S. Li, et al., Chem. Eng. J. 489 (2024) 151412. doi: 10.1016/j.cej.2024.151412

    205. [205]

      J.Z. Li, H.G. Zhang, W. Samarakoon, et al., Angew. Chem. Int. Ed. 58 (2019) 18971–18980. doi: 10.1002/anie.201909312

    206. [206]

      Y. Yuan, Q. Zhang, L. Yang, et al., Adv. Funct. Mater. 32 (2022) 2206081. doi: 10.1002/adfm.202206081

    207. [207]

      Y.C. Zeng, C.Z. Li, B.Y. Li, et al., Nat. Catal. 6 (2023) 1215–1227. doi: 10.1038/s41929-023-01062-8

    208. [208]

      K. Muñoz-Becerra, R. Venegas, L. Duque, et al., Curr. Opin. Electrochem. 23 (2020) 154–161. doi: 10.1016/j.coelec.2020.08.006

    209. [209]

      J. Li, M.T. Sougrati, A. Zitolo, et al., Nat. Catal. 4 (2021) 10–19. doi: 10.18282/l-e.v10i2.2248

    210. [210]

      J. Yang, Z.Y. Wang, C.X. Huang, et al., Angew. Chem. Int. Ed. 60 (2021) 22722–22728. doi: 10.1002/anie.202109058

    211. [211]

      Y.Z. Wang, T.M. Yang, X. Fan, et al., Angew. Chem. Int. Ed. 63 (2024) e202313034. doi: 10.1002/anie.202313034

    212. [212]

      S. Zhu, L.T. Ding, X.H. Zhang, et al., Angew. Chem. Int. Ed. 62 (2023) e202309545. doi: 10.1002/anie.202309545

    213. [213]

      Y. Wang, Z. Bao, M. Shi, et al., Chemistry 28 (2022) e202102915. doi: 10.1002/chem.202102915

    214. [214]

      R. Gao, J. Wang, Z.-F. Huang, et al., Nat. Energy 6 (2021) 614–623. doi: 10.1038/s41560-021-00826-5

    215. [215]

      X.Y. Zhou, Z.Y. Jin, J.Z. Zhang, et al., Nanoscale 15 (2023) 2276–2284. doi: 10.1039/d2nr05974f

    216. [216]

      H. Hu, P. Zhang, B.B. Xiao, et al., ACS Appl. Mater. Interfaces 15 (2023) 23170–23184. doi: 10.1021/acsami.3c02232

    217. [217]

      R. Zeng, Y. Yang, X. Feng, et al., Sci. Adv. 8 (2022) eabj1584. doi: 10.1126/sciadv.abj1584

    218. [218]

      R. Zeng, H. Li, Z. Shi, et al., Nat. Mater. 23 (2024) 1695–1703. doi: 10.1038/s41563-024-01998-7

    219. [219]

      J. Kim, W. Ko, J.M. Yoo, et al., Adv. Mater. 34 (2022) 2107868. doi: 10.1002/adma.202107868

    220. [220]

      L. An, Y. Hu, J. Li, et al., Adv. Mater. 34 (2022) 2202874. doi: 10.1002/adma.202202874

    221. [221]

      J.J. Huang, Y. Yang, D. Weinstock, et al., Nat. Catal. 8 (2025) 116–125. doi: 10.1038/s41929-025-01289-7

    222. [222]

      Y. Yang, Y. Xiong, M.E. Holtz, et al., Proc. Natl. Acad. Sci 116 (2019) 24425–24432. doi: 10.1073/pnas.1906570116

    223. [223]

      Y. Wang, Y. Yang, S. Jia, et al., Nat. Commun. 10 (2019) 1506. doi: 10.1038/s41467-019-09503-4

    224. [224]

      Y. Sun, T. Zhang, P. Sun, et al., J. Energy Chem. 94 (2024) 778–788. doi: 10.1080/00223131.2023.2269974

    225. [225]

      J.L. Rowell, A. Joshi, H. Tan, et al., ACS Catal. 15 (2025) 9738–9748. doi: 10.1021/acscatal.5c00896

    226. [226]

      M. Yoo, E. Kang, H. Choi, et al., J. Mater. Chem. A 10 (2022) 5942–5952. doi: 10.1039/d1ta08059h

    227. [227]

      Z. Xue, H. Song, J.A. Rogers, et al., Adv. Mater. 32 (2020) 1902254. doi: 10.1002/adma.201902254

    228. [228]

      Z. Du, L. Shen, Y. Gong, et al., Adv. Energy Mater. 34 (2024) 2310790. doi: 10.1002/aenm.202310790

  • Figure 1  Schematic diagram of strain engineering and ORR catalysts.

    Figure 2  4e− and 2e− processes of ORR with association and dissociation pathway diagram.

    Figure 3  Correlation between strain effects and d-band center characteristics. (a, b) Schematic representations demonstrating tensile strain's impact on d-orbital alignment in early/late transition metal systems. Reproduced with permission [50]. Copyright 2017, Springer Nature. (c) Visualization depicting Pt-Pt interatomic spacing and interfacial geometry in Pt-skin/intermetallic core structures. (d) Comparative analysis of calculated versus measured overpotentials for various intermetallic compositions relative to Pt's d-band center position. Reproduced with permission [52]. Copyright 2023, Wiley-VCH. (e) Thermodynamic potential profile diagram. (f) Computational modeling of overpotential variations with applied tensile strain on ordered PtNi surfaces Reproduced with permission [54]. Copyright 2020, American Chemical Society.

    Figure 4  Strategies to induce strain. (a) Schematics of strain-enhanced Pt-Co bimetallic solid solutions. Reproduced with permission [55]. Copyright 2024, Springer. (b) Illustration of lattice mismatched epitaxy introduced compressive strain in core-shell nanoparticles. Reproduced with permission [56]. Copyright 2019, American Chemical Society. (c) Visual explanations of lattice deformation mechanisms, adsorbate-transition metal interactions, and upward shifts in d-band center positions. Reproduced with permission [58]. Copyright 2024, Wiley-VCH. (d) Surface strain caused by particle size/shape. Reproduced with permission [56]. Copyright 2019, American Chemical Society. (e) Strain formation at crystalline interface boundaries or structural defects (hole). (f) Surface curvature effect caused strain. Reproduced with permission [57]. Copyright 2023, American Chemical Society.

    Figure 5  Strain in alloys. (a) Schematic illustration of strain effect in PtM alloy. Reproduced with permission [59]. Copyright 2023, American Chemical Society. (b) HAADF-STEM images of Pt56Mn44 nano-dendrites. (c) XPS spectra of Pt 4f orbitals alongside EXAFS evaluations at the Pt L3 absorption edge and (d) multiscale wavelet transformation patterns. (e) Comparative Tafel slope analysis, (f) ORR catalytic metrics including SA and MA (0.9 V vs. RHE) across various electrocatalysts. Reproduced with permission [66]. Copyright 2024, Wiley-VCH. (g) Activity-structure correlations mapping mass performance against Pt-Pt bond distances in PtMnM/C versus PtMn/C systems. (h) Electronic parameter relationships connecting catalytic activity with d-band center positions. (i) Mechanistic illustration of strain/electronic configuration impacts on intermediate adsorption in PtMnM alloys. (j) Performance benchmarking of PtMnCo/C against conventional catalysts through MA/SA measurements. Reproduced with permission [68]. Copyright 2024, Science China Press. (k) AC-STEM images and the corresponding GPA images for axial strain (εxx) and shear strain (εxy). (l) Bader charge analysis and (m) the d-band center of different elements in HEANs. (n) ORR polarization of Tafel plots, and onset potential at 1600 rpm for HEAN/CNT and Pt/C. Reproduced with permission [71]. Copyright 2024, the Author(s).

    Figure 6  Strain in core-shell catalysts. (a) Fourier-transformed k3-weighted Pt L-edge XANES spectra and (b) wavelet analysis patterns for FePt@PtBi systems, compared to FePt and Pt/C reference materials. (c) Chromatic mapping illustrating lattice distortion patterns across Pt, FePt, and FePt@PtBi structures Reproduced with permission [77]. Copyright 2021, Wiley-VCH. (d) Structural model demonstrating strain distribution in fct-PtCo@PtIr/C heterostructures. (e) GPA strain image. (f) Catalytic performance metrics showing mass-normalized and surface-specific activities at 0.9 V vs. RHE Reproduced with permission [79]. Copyright 2023, Wiley-VCH. (g) Synthetic process of Se2-Pt NPs and corresponding structural evolution on the surface. Surface structures of Se1-Pt NPs and Se3-Pt NPs. (h) The d-band centers of the active-site Pt atoms in various catalysts. (i) The 2e−/4e− ORR path and corresponding energy barriers for Se2-Pt and Se3-Pt. (j) Values of the selectivity (%). Reproduced with permission [81]. Copyright 2024, Nature. (k) Atomic-resolution HAADF-STEM and (l) HRTEM micrographs of mesoporous Pt@Pt-skin Pt3Ni core-shell frameworks. (m) Diffraction intensity comparisons between bulk Pt (111) planes and Pt-skin surfaces revealing ~4.9% compressive lattice strain. MA and SA variations observed in the mesoporous Pt@Pt-skin Pt3Ni CSFWs/C electrocatalyst. Reproduced with permission [82]. Copyright 2023, Nature.

    Figure 7  Strain effects based on size/shape characteristics. (a) Structural diagrams of fcc-PtCo, fct-PtCo/C, and fct-PtCo@Pt/C catalysts, along with their corresponding (b) XRD diffraction profiles. (c) Catalytic performance metrics showing MA comparisons. Reproduced with permission [87]. Copyright 2021, American Chemical Society. (d) Average particle size (indicated by black lines) and (e) MA and SA measurements for PtMo/C-X catalysts synthesized at varying temperatures (200-1000 ℃). Reproduced with permission [92]. Copyright 2022, American Chemical Society. (f) Architectural visualization of the CS-Pt/C catalyst system. (g) Computed surface strain patterns and *OH adsorption energy simulations on Pt cone. (h) LSV profiles during accelerated durability testing cycles, comparing the MA and SA of CS-Pt/C catalysts pre- and post-stability evaluations. Reproduced with permission [93]. Copyright 2024, Wiley-VCH. Mechanistic representations of 2e− ORR toward hydrogen peroxide generation using (i) S- and (j) L-ZnO nanoplate catalysts. AFM topographic mappings with elevation analyses for (k) S- and (l) L-ZnO nanoplates along designated transects. (m) Comparative Gibbs free energy variations and (n) electronic density of states (DOS) characteristics for S- versus L-ZnO configurations during 2e− ORR processes. Reproduced with permission [94]. Copyright 2023, Royal Society of Chemistry.

    Figure 8  Strain by defects. (a) The relationship between surface stress release and surface strain generation of stepped Pt (111) surfaces. (b) Side view (upper panels) and atomic site-resolved surface strain (lower panels) of Pt (332), and (c) Pt (21 21 20) surfaces with terrace width from 1.3 nm (n = 5) to 10.1 nm (n = 41), as indicated by double arrow lines. Surface sites correspond to atoms in the top layer of the side views. (d) Side view (upper panels) and atomic site-resolved d-band center shift (dεd), (e) OH adsorption energy shift and predicted ORR improvement factors of Pt (21 21 20) surfaces with respect to that of the Pt (111) surface. Reproduced with permission [48]. Copyright 2024, Nature. (f) Diagram of the relationship between atomic arrangement and (g) coordinative shell, atomic PDFs of Vac-NiPt, NPs/NG, Vac-Pt NPs/NG and commercial Pt/C. (h) Histogram about kinetic current density, SA and MA of Vac-NiPt NPs/NG, Vac-Pt NPs/NG, and Pt/C at 1600 rpm and -0.85 V vs. RHE. (i) Negatively polarized LSV curves of Vac-NiPt NPs/NG and Pt/C before and after 50 k, 100 k and 200 k cycles Reproduced with permission [101]. Copyright 2025, Wiley-VCH.

    Figure 9  Strain by substrate. (a) High-resolution TEM of Fe-N-hcC. (b) Fourier transformed Fe K-edge EXAFS spectra for Fe-N-C, Fe-N-hcC, and related reference compounds. (c) Correlations between the d-band center for the single Fe sites in FeN4 and the ΔGOH*. (d) Mass activities and TOF values at 0.85 V for the Fe-N-hcC and Fe-N-C electrocatalysts. Reproduced with permission [110]. Copyright 2023, Wiley-VCH. (e) Schematic of the Co-WC structure with both Co superstructure formation. (f) Bonding status and adsorption behavior under pristine (blue) and compressive (red) stress. (g) The stress-induced changes in Co-C bond length. (h) Theoretical overpotential of the catalyst for OER and ORR under different stresses. (i) Bifunctional LSV curves of Co/WC and Pt/C+IrO2 in an O2-saturated 0.1 mol/L KOH solution. Reproduced with permission [111]. Copyright 2024, American Chemical Society.

    Figure 10  Strain analysis of substrate curvature. (a) Depiction of structural deformations in CoPc when deposited on CNTs with varying diameters. (b) EXAFS Fourier analysis comparing CoPc/SWCNTs with CoPc/15, CoPc/50 and pristine CoPc. (c) Comparative analysis of E1/2 values and mean electron transfer counts for FePc/SWCNT, FePc/15, FePc/50 versus commercial Pt/C in oxygenated 0.1 mol/L KOH solution. Reproduced with permission [112]. Copyright 2023, Nature. (d) Thermodynamic free energy comparison between planar and curved FePc-C24 configurations under 0.0, +0.8, and +1.0 V potentials at 298 K. (e) ORR LSV profiles demonstrating durability after 5000 CV cycles for FePc/SWCNT versus 20% Pt/C. Reproduced with permission [113]. Copyright 2025, American Chemical Society. (f) E1/2 performance comparison. (g) Electrochemical stability evaluation of HCNT, Co-N-C@CNT, Co-N-C@HCNT and Pt/C at 1600 rpm in alkaline oxygen environment. (h) Power output characteristics and discharge profiles comparing Co-N-C@HCNT with Pt/RuO2 composite. Reproduced with permission [114]. Copyright 2024, Wiley-VCH.

    Figure 11  Strain in Pt-based alloys. (a) HR-TEM image of PtCo/C-600 ℃. (b) Variation of Pt-Pt bond lengths for different models along the (110) direction. (c) PDOSs and d-band centers of Pt (110) and models with localized strains. (d) Steady-state polarization curves after 30,000 cycles of ADT. Reproduced with permission [127]. Copyright 2024, Wiley-VCH. (e) ∆EO as a function of compressive strain on the (111) surface. The horizontal red line indicates the optimal value of ∆EO. (f) Comparative electrocatalytic metrics including MA and SA values at 0.9 V (vs. RHE) for S-PtCo SNPs/C, S-Pt3Co SNPs/C, and benchmark Pt/C catalyst. Reproduced with permission [55]. Copyright 2024, Springer. (g) Evolution of surface Pt d-band center during structural transformations. (h) Performance comparison of Pt-based catalysts (Pt/C, Pt3Co/C, Rh-Pt3Co/C) at 0.9 V operating potential. (i) Voltage stability assessment at 0.8 A/cm2 current density before and after electrochemical aging tests. Reproduced with permission [128]. Copyright 2024, Wiley-VCH.

    Figure 12  Strain in ternary Pt alloys. (a) Correlation between Cu concentration and measured strain percentages obtained through XRD analysis and HRTEM visualization. (b) Comparative evaluation of nanoparticle dimensions calculated through XRD and TEM techniques across varying Cu compositions. (c) Interdependent relationships among ECSA, MA, SA, and lattice contraction effects relative to ternary alloy nanoparticle dimensions. Reproduced with permission [129]. Copyright 2023, Wiley-VCH. (d) Sequential fabrication steps for PtNiW/C catalyst production. (e) Atomic-resolution HAADF-STEM visualization with dimeric Ni-O-W coordination analysis through intensity profiling and two-dimensional strain distribution mapping via geometric phase analysis. (f) Corresponding K3-weighted magnitude of Fourier transform spectra from EXAFS. (g) PDOS of Pt-d orbitals in Pt foil, PtNi/C, PtW/C and PtNiW/C, including the ϵ values. (h) Mass activities at 0.9 V vs. RHE of four catalysts before stability (pure color) and after stability (gradient color). Reproduced with permission [130]. Copyright 2024, Wiley-VCH.

    Figure 13  Strain in Pt-based HEA. (a) The illustration of the surface strain (ɛsurf) originated from the lattice mismatch of the interface between the intermetallic/alloy core and Pt shell. The schematic illustration of the machine learning-guided element selection process toward low-Pt ORR catalysts. The area surrounded by the gray line represents the crystal graph convolutional neural networks (CGCNN) model. (b) Comparative catalytic performance metrics (mass/specific activity) measured at 0.9 V relative to RHE. (c) Correlation analysis between specific activity values and ɛsurf parameters. Reproduced with permission [135]. Copyright 2025, Wiley-VCH. (d) The calculated PDOS of Pt 5dz2 electrons. The gray, blue, and red lines stand for the d-band centers of pure Pt slab, Pt/HEA, and N/Pt/HEA, respectively. (e) Mass and specific activity (0.9 V vs. RHE) of N/Pt/HEA NPs-C, Pt/HEA NPs-C, and Com Pt-C catalysts. Reproduced with permission [136]. Copyright 2025, Elsevier. (f) EXAFS spectra of the E/O-PtFeCoNiMn/C catalyst and standard Pt foil in R-space. (g) The calculated DOS of Pt (111) and PtFeCoNiMn (111). (h) Calculated mass and specific activity at 0.9 V for ORR for E/O-PtFeCoNiMn/C and Pt/C catalysts. Reproduced with permission [137]. Copyright 2024, Elsevier.

    Figure 14  Strain effects in platinum intermetallic compounds. (a) HAADF-STEM characterization of Pt3Ga (Pm3m) and Pt3Ga (P4/mbm) phases, with atomic structural models illustrating their orientation relative to the Pt (110) reference plane. (b) Correlation plot showing the interdependence of *O intermediate adsorption free energy, overpotential, and lattice compression characteristics on Pt surfaces. (c) Projected density of states analysis for Pt atoms bonded with *OH species in Pt3Ga (Pm3m). (d) Comparative evaluation of MA and SA at 0.9 V vs. RHE for PtGa alloys, Pt3Ga polymorphs, and commercial Pt/C catalysts. Reproduced with permission [143]. Copyright 2024, Wiley-VCH. (e) Atomic-resolution HAADF-STEM visualization of L10-Pt2CuGa nanoparticles, with inset fast Fourier transform pattern. (f) Comparative Pt L3-edge EXAFS Fourier transforms for L10-Pt2CuGa/C, L11-PtCu/C, and metallic Pt references. (g) Activity-structure relationship mapping between ORR specific activity and Pt-Pt bond distances. (h) Comparative analysis of vacancy formation energies for Pt (111) surfaces versus L10-Pt2CuGa systems. (i) ADT results showing ORR polarization curves for L10-Pt2CuGa/C before and after potential cycling. (j) Performance metrics tracking MA retention and hydrogen-oxygen fuel cell peak power output during stability assessments. Reproduced with permission [148]. Copyright 2024, Wiley-VCH. (k) Relation between strain, d-band center, and ORR free energy barrier of L10-GaPtCo, A1-PtCo, and Pt. (l) MA at 0.9 V in H2-O2 fuel cells and the voltage at 0.8 A/cm2 in H2-air fuel cells before and after AST test. Reproduced with permission [149]. Copyright 2023, Nature.

    Figure 15  Strain in Pt core-shell. (a) Surface strains of PdRD@Pt nL NCs along the two in-plane directions. (b) Specific and mass activities of different catalysts at 0.9 V vs. RHE. Reproduced with permission [153]. Copyright 2022, American Chemical Society. (c) Optimized configuration of Pt48Ag45Pb3 (111), Pt51Ag33Pb12 (110), and Pt55Ag19Pb22 (110) NCs image, (d) maps of the in-plan strain tensors εxx, εyy, εxy, processed via GPA taken from the yellow frame area. (e) PDOS for Pt and Pb atoms within Pt51Ag33Pb12 (110) and Pt55Ag19Pb22 (110) nanocrystal systems. Reproduced with permission [154]. Copyright 2022, Wiley-VCH. (f) Free energy profiles. (g) Correlation between tensile strain in platinum nanoparticles and incorporated nitrogen atom quantities. (h) MA variations across catalyst materials before and after 20,000 electrochemical cycles. Reproduced with permission [155]. Copyright 2020, Elsevier. (i) ORR enhancement (lower panel) and associated tensile strains (upper panel) relative to third-layer zirconium deposition thickness in Pt-shell configurations. Reproduced with permission [156]. Copyright 2019, American Chemical Society.

    Figure 16  Strain in Pd-based alloys. (a) TEM images paired with dilatational strain distributions for (a1) Exx, (a2) Exy and (a3) rotational strain patterns observed in Pd6Au HSs. (b) Corresponding TEM visualizations with (b1) Exx, (b2) Exy strain mappings and (b3) rotational strain profiles for Pd3Au HSs. (c, d) Quantitative analysis showing strain center density (/nm2, exx) correlations with E1/2 in PdAu HSs. Reproduced with permission [159]. Copyright 2020, Elsevier. (e) Current-time profiles comparing electrochemical stability of Pd4Au HSs/C, Pd4Au HCs/C, and commercial Pt/C catalysts at 0.6 V versus RHE. (f) Performance metrics illustrating MA and SA comparisons at 0.85 V vs. RHE. (g) Schematic illustration of synthetic methodology for PdAu HCs. (h) TEM characterization of Pd4Au HCs with GPA-derived strain mappings. Color-coded dilatational strain (εxx) distributions (green-dark blue indicating compression, red-yellow representing tension) and rotational strain patterns. Reproduced with permission [160]. Copyright 2020, Wiley-VCH.

    Figure 17  Strain in PdMo alloys. (a) Left panel displays the lateral perspective of the nanoscale architecture in four-layered PdMo bimetallene. Right panel illustrates the planar configuration highlighting atomic arrangements in layers 2-3. (b) Variations in the ∆EO parameter for PdMo bimetallene under different mechanical loading conditions (compression vs. tension). A reference threshold value is marked by the crimson horizontal indicator. (c) PDOS analysis for surface Pd atoms across bulk palladium, four-layer Pd nanosheets (Pd 4L), and Pd-Mo composites. Dashed horizontal markers denote computed d-band central positions. Reproduced with permission [161]. Copyright 2019, Nature. (d) CV curve of PdMo recorded in a 0.1 mol/L HClO4 electrolyte. (e) Magnified image of the (111) diffraction peak as highlighted with a rectangle. (f) Micro-strain calculated from WAXS data using the W-H method. (g) Site-dependent PDOSs of Pd-4d and (h) Mo-4d orbitals in PdMo-H10m. (i) Adsorption energy and charge comparisons of *O2. (j) Reaction energy of the ORR under U = 0 V. (k) Comparison of SA and E1/2 for PdMo, PdMo-H10m, and PdMo-H. Reproduced with permission [163]. Copyright 2024, American Chemical Society.

    Figure 18  Strain in Pd HEA. (a) Preparation of Pd@PdBiCo MAs. (b) Comparison of E1/2 and mass activity of the commercial Pd/C, Pd MAs/C, and Pd@PdBiCo MAs/C. (c) HRTEM images of Pd@PdBiCo MAs and (d) Pd MAs. (e) Integrated pixel intensified of Pd (111) lattices and (f) PXRD patterns of Pd@PdBiCo MAs and Pd MAs. Reproduced with permission [164]. Copyright 2023, Wiley-VCH. (g1) High-magnification TEM; (g2) FFT-derived crystallographic orientation; (g3) Strain mapping visualization; (g4) Quantitative strain measurement across particle diameter (compressive strain denoted by negative values) [166]. (h) Comparative strain analysis among PdCuMoNiCo NHSs, ternary/quaternary alloys, and pure Pd. (i) Normalized MA_SA at 0.8 V vs. RHE. Reproduced with permission [167]. Copyright 2022, Royal Society of Chemistry. (j) Catalytic performance benchmarking of 5-Pd-HECs/C against Pd-NCs/C and commercial Pt/C at 0.9 V vs. RHE. Reproduced with permission [166]. Copyright 2024, Royal Society of Chemistry.

    Figure 19  Strain in Pd nanomesh. (a1) Magnified HAADF-STEM visualization of the perforation's interior margin (yellow frame). (a2) Cumulative intensity profiles across Pd (200) crystalline planes. (a3) Strain field mapping through geometric phase analysis (eyy component) corresponding to the zoomed Area 1. (b1) High-resolution HAADF-STEM examination of the mesh periphery (red frame). (b2) Integrated intensity distribution along Pd (111) crystallographic planes from Fig. 2f. (b3) GPA-derived strain mapping (eyy component) for Area 2, with chromatic scale indicating -20% to +20% strain variation. (c1) Surface structural configurations (m1-m4) in plan view. (c2) Catalytic activity profiles comparing *OH (black) and *OOH (green) adsorption energies for 4e− pathways. c3) Comparative d-orbital electronic structures with vertical markers indicating d-band center positions. (d) MA versus SA performance metrics at 0.9 V RHE. (e) Volumetric current density at 0.6 V and maximum power output characteristics. Reproduced with permission [170]. Copyright 2025, Wiley-VCH.

    Figure 20  Strain in other noble metal catalysts. (a) Schematic illustration depicting the strained RuO2 structure. (b) XANES spectra at the Ru K-edge and (c) Fourier-transformed EXAFS spectra derived from k2-weighted data for Ru/RuO2@NCS, RuO2, and metallic Ru references. (d) Correlation between lattice strain in RuO2 and adsorption free energy of 2*O species. Electronic structure comparison through PDOS analysis for (e) unmodified RuO2 and (f) strain-engineered RuO2. (g) Electrochemical characterization showing ORR Tafel plots, limiting-current densities, and E1/2. (h) ORR durability test. Reproduced with permission [174]. Copyright 2022, Wiley-VCH. (i) Diagram for tailoring atomic strain of Fe sites by second metal atoms. (j) Fe Mossbauer spectrum of Ru/Fe-N-C. (k) Bar chart showing Eonset and E1/2 of Ru /Fe-N-C and the kinetic current density at 0.85 and 0.8 V. Reproduced with permission [175]. Copyright 2024, Elsevier.

    Figure 21  Strain in Au/Ag-based catalysts. (a) High resolution HAADF-STEM micrograph of the GBs between the Au NP building blocks within H-Au NAs. (b) Real space strain maps along the x (εxx), y (εyy) and xy (εxy) directions. (c) Relationship between gas flow rates and GB surface density. (d) Correlation between GB surface density and lattice expansion/coordination number calculated from the Fourier-transformed EXAFS spectra. (e) Calculated H2O2 selectivity during potential sweep. (f) Correlation between GB density and the 2e− ORR activity, including onset potential, H2O2 selectivity, specific activity, and mass activity. Reproduced with permission [180]. Copyright 2024, Nature. (g) Raman spectra of Ag2Mo2O7 samples. (h) Electron localization function on (020) and (1¯02) planes of AMO2. (i) Shift of Mo d-band center, Ag d-band center, and O p-band center after coordination rearrangement. (j) PDOS of Mo 4d and O 2p orbitals. (k) PDOS of Ag 4d orbitals. Reproduced with permission [181]. Copyright 2024, Wiley-VCH.

    Figure 22  Strain in metal-free carbon catalyst. (a) Structural comparison between P-A-GN and C-A-GN configurations, visualized using an iso-surface value of 0.0005 e/Å3. (b) Electrochemical characterization showing Tafel plot variations and (c) ORR polarization curves (1600 rpm) for CNRs-C samples under O2-saturated 0.1 mol/L KOH before and after 10,000 stability cycles. Reproduced with permission [190]. Copyright 2023, Wiley-VCH. (d) Experimentally determined structural parameters including C-O bond distances and C-O-C angular configurations. (e) Schematic representation of curvature-modified carbon surfaces. (f) Charge redistribution patterns visualized through differential density analysis (yellow: electron accumulation; cyan: depletion; iso-surface = 0.005 e/Bohr3). (g) Correlation between the Bader charges at the two neighboring C atoms and the O atoms and the C p-band center to R. (h) Performance comparison with recent reports. Reproduced with permission [193]. Copyright 2024, American Chemical Society. (i) Half Violin plots of overpotential for SWG-O sites. (j) Correlation between tensile strain and ORR current density at 0.05 V vs. RHE. (k) Structures of graphene models with various defects, MVG, DVG, and SWG. MVG, DVG, and SWG refer to the graphene nanoribbon with a monovacancy, divacancy, and Stone-Wales defect, respectively. (l) ORR polarization curves of pristine HOPG under different tensile strains ε from 0.0% to ~ 2.1%. (m) ORR polarization curves of D-HOPG under different tensile strains ε from 0.0% to ~ 2.4%. Reproduced with permission [194]. Copyright 2025, American Chemical Society.

    Figure 23  Strain in M-N-C catalysts. (a) XANES spectra of different catalysts. (b) Structural configurations and electron density distributions in FeN4 active sites under both relaxed conditions and 2% Fe-N bond contraction scenarios. (c) Electronic state analysis through Fe 3d orbital density of states for contrasting FeN4 configurations. Reproduced with permission [205]. Copyright 2019, Wiley-VCH. (d) Design schematic illustrating the FeCoNP@FeSA-N/C composite catalyst architecture. (e) Comparative free energy profiles and reaction pathways for catalytic processes, with RDS clearly identified. Reproduced with permission [206]. Copyright 2022, Wiley-VCH. (f) Durability assessment showing performance evolution of Fe-N-C catalysts under accelerated stress testing (30,000 AST cycles) across varied atmospheric conditions. (g) Synthetic strategy visualization for creating S1/S2 active sites through controlled pyrolysis environments. (h) Real-space (R-space) Fourier transforms of EXAFS data. (i) Reciprocal space (κ-space) EXAFS fitting comparisons for Fe-N-C-Ar, Fe-N-C-10%FG, and iron phthalocyanine references. Reproduced with permission [207]. Copyright 2023, Nature.

    Figure 24  Strain in curved M-N-C catalysts. (a) Fabrication procedure for D-Fe SAC. (b) EXAFS analysis outcomes comparing D-Fe SAC with LD-Fe SAC. (c) Electrochemical performance metrics including E1/2 and kinetic current densities (0.9 V vs. RHE) across catalyst variants. Reproduced with permission [210]. Copyright 2021, Wiley-VCH. (d) Schematic representation depicting the synthesis pathway for FeNS/Fe3C@CNS. (e) Comparative Tafel slope measurements among FeNS/Fe3C@CNS, FeN/Fe3C@CNS, CNS, CNT@Fe and Pt/C in 0.1 mol/L HClO4 electrolyte under O2 saturation. (f) Chronoamperometric stability profiles of FeNS/Fe3C@CNS versus Pt/C in acidic media. Reproduced with permission [211]. Copyright 2024, Wiley-VCH. (g) Preparation methodology illustration for FePc-{PW12}@NT and FePc-{PW12}/NT catalytic systems. (h) Electron density distribution patterns in FePc-NT versus FePc-{PW12}@NT (isosurface level: 0.0005). (i) Comparative free energy profiles for ORR mechanisms across FePc-{PW12}@NT, FePc-NT and FePc configurations. (j) Catalytic activity indicators showing kinetic current densities (JK) at 0.8 V and corresponding E1/2. Reproduced with permission [212]. Copyright 2023, Wiley-VCH.

    Figure 25  DFT prediction of strain in M-N-C. (a) The strain energy change with increasing m of Co-N-CNTs. (b) EOH as a linear relationship between the d-band center of Co atom in Co-N-CNTs. (c) ΔG*OH as a function of m of Co-N-CNTs. Reproduced with permission [215]. Copyright 2023, Elsevier. (d) Height (hSn) and the apex angle (θ) of the Sn-N4 square pyramid (depicted in the inset) of Sn-N-CNTs and Sn-N-GQDs. Tensile strain εSn applied to the Sn-N4 pyramid of Sn-N4-CNTs and the compressive strain εSn applied to the Sn-N4 pyramid of Sn-N4-GQDs (taken Sn-N4 of Sn-N4-Gra as the equilibrium state), as schematically illustrated in the inset. (e) ΔG*OOH-ΔG*O versus ΔG*OH on Sn-N-CNTs. (f) Volcano plot relationship between ΔG*OH and the calculated overpotential of ORR. Reproduced with permission [216]. Copyright 2023, American Chemical Society.

    Figure 26  Strain in transition metal nitride/oxide. (a) Schematic synthesis procedure of metal nitrides (MxN) supported on high-surface area carbon via nitridation with ammonia. (b) Comparison of the MA of all MxN/C measured at 0.85 V vs. RHE. Reproduced with permission [217]. Copyright 2022,Wiley-VCH. (c) Schematic atomic model of Mn3O4 shell and MnN core structure along MnN [100] and MnN [110]. (d) Atomic-resolution image of MnN along the [110] projection and Mn3O4 along the [100] projection. (e) In-plane strain measurements from the atom layers in (d). Reproduced with permission [218]. Copyright 2024, Nature. (f) Structural transformation of MMO spinel catalyst Reproduced with permission [219]. Copyright 2022, Wiley-VCH. (g) Computed nanoparticle strain variations versus electrochemical potential. (h) Cyclic voltammetry current profile (green) with corresponding strain responses during cathodic (red) and anodic (blue) potential sweeps. (i) Mechanical model visualization depicting adsorbate-induced surface stress in nanoparticle analogs to pressurized thin-walled containers. (j) CV current trace spanning 0.05-1.4 V (green) with concurrent strain measurements. Reproduced with permission [221]. Copyright 2025, Nature.

    Figure 27  Strain in spinel/perovskite catalysts. (a) Half-wave potential for 1 to 5 CMO shell samples, CMO and Pt/C. (b) Half-wave potential vs. lattice constant and (c) mass activity vs. lattice constant for 1 to 5 CMO shell samples. Reproduced with permission [225]. Copyright 2025, American Chemical Society. (d) Structural representations of PBSCF-c and BSCFW-c crystalline phases. (e) Temperature-dependent lattice mismatch evolution between PBSCF-c and BSCFW-c polymorphs. (f) Electrochemical impedance spectra (normalized by active surface area) for symmetrical half-cells employing BSPCFW electrodes. (g) Comparative polarization resistance (Rp) values for PBSCF, PBSCF-s, and BSPCFW cathodes under varying thermal conditions. (h) Long-term Rp stability assessment of symmetrical cells with PBSCF and BSPCFW electrodes at 650 ℃ operational temperature. Reproduced with permission [228]. Copyright 2024, Wiley-VCH.

    Table 1.  Comparison of different strain.

    Strain type Generation mechanism Typical catalyst Strain regulation range Influence on ORR activity References
    Strain of alloy structure Differences in atomic radii of mixed metals Pt56Mn44/C;
    Rh-Pt3Co/C;
    -0.43%;
    -2.9%
    MA = 0.53 A/mgPt
    SA = 1.0 mA/cm2;
    MA = 1.31 A/mgPt,
    SA = 1.77 mA/cm2;
    [66];
    [128]
    Strain of core-shell structure Lattice mismatch between core and shell Pt @Pt-skin Pt3Ni CSFWs;
    fct-PtCo @PtIr/C
    -4.9%;
    -1%~-3%
    MA = 6.69 A/mgPt
    SA = 8.42 mA/cm2;
    MA = 1.17 A/mgPt+Ir
    SA = 2.63 mA/cm2Pt+Ir
    [82];
    [79]
    Strain caused by the size and shape change Increased specific surface area of nanoparticles CS-Pt/C (2 nm);
    PtCoCu (2.98-10.9 nm)
    -0.5%~-2.5%;
    -2.38%~-2.84%
    MA = 1.72 A/mgPt
    SA = 0.99 mA/cm2;
    MA = 1.19 A/mgPt
    SA = 1.48 mA/cm2;
    [93];
    [129]
    Strain caused by defects Defects (vacancies, steps) Pt (21 21 20);
    the defective HOPG;
    -3.7% (step)
    -0.3% (terrace);
    +0.6%
    50 times (ORR improvement factor);
    35% (current density increased)
    [48];
    [194]
    Strain caused by the substrate Strong interactions at the metal-support interface Co-WC;
    BSPCFW
    -5%;
    +2%~+3%
    0.45 V (overpotential)
    E1/2 = 0.893 V vs. RHE;
    Rp = 0.068 Ω cm2 (600 ℃)
    [111];
    [228]
    下载: 导出CSV
  • 加载中
计量
  • PDF下载量:  4
  • 文章访问数:  144
  • HTML全文浏览量:  9
文章相关
  • 发布日期:  2027-01-12
  • 收稿日期:  2025-08-23
  • 接受日期:  2025-10-21
  • 修回日期:  2025-10-16
  • 网络出版日期:  2025-10-22
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

/

返回文章