纳米氧化铜-碳纳米管修饰玻碳电极同时检测邻、对苯二酚

常凤霞 ,  尚宗毅 ,  董清 ,  龙志彦 ,  邓怡雪

引用本文: 常凤霞, 尚宗毅, 董清, 龙志彦, 邓怡雪. 纳米氧化铜-碳纳米管修饰玻碳电极同时检测邻、对苯二酚[J]. 应用化学, 2020, 37(10): 1195-1202. doi: 10.11944/j.issn.1000-0518.2020.10.200048 shu
Citation:  CHANG Fengxia, SHANG Zongyi, DONG Qing, LONG Zhiyan, DENG Yixue. Simultaneous Determination of Catechol and Hydroquinone by Copper Oxide Nanoparticles and Carbon Nanotubes Modified Glassy Carbon Electrode[J]. Chinese Journal of Applied Chemistry, 2020, 37(10): 1195-1202. doi: 10.11944/j.issn.1000-0518.2020.10.200048 shu

纳米氧化铜-碳纳米管修饰玻碳电极同时检测邻、对苯二酚

    通讯作者: 常凤霞, 讲师; Tel/Fax:028-85928021;E-mail:changfengxia@swun.edu.cn; 研究方向:电化学传感和整流
  • 基金项目:

    西南民族大学中央高校基本科研业务费专项基金(2020NQN07)项目资助

摘要: 以商品化纳米氧化铜和羧化碳纳米管作为玻碳电极修饰材料,结合了两种材料的放大电信号和电催化性能,所构建的复合物修饰电极可区分性质相近的同分异构体邻苯二酚和对苯二酚的信号,同时可进一步放大两种酚的峰电流。因此该基于纳米氧化铜和碳纳米管的电化学传感器可用于邻苯二酚和对苯二酚的同时检测。采用循环伏安法对复合物中两种材料的比例、修饰量以及支持电解质pH进行了优化:纳米氧化铜和碳纳米管质量比为5:1,修饰量为9 μL,pH=7.4的磷酸盐缓冲溶液被用作电解质溶液。在优化的条件下,邻苯二酚和对苯二酚的微分脉冲伏安扫描峰电流与浓度在6.0×10-7~3.0×10-3 mol/L范围内均呈良好的线性关系,检出限(S/N=3)分别为1.0×10-7和1.6×10-7 mol/L。该方法具有成本低、操作简便、快速的特点,对实际水样的加标回收率在94.6%~101.1%范围内,具有较好的实际应用前景。

English

  • 邻苯二酚(Catechol, CC)和对苯二酚(Hydroquinone,HQ)是重要的化工中间体和原料,在橡胶、电镀、显影剂、染料、阻聚剂和涂料等工业中被广泛应用。CC和HQ结构和性质相近,常共存于工业污水中,因为具有毒性及低降解性,是具有较大危害的环境污染物[1-3]。因此对邻苯二酚和对苯二酚的高选择性、高灵敏度的同时检测在环境监测和治理领域具有重要的现实意义。目前,已发展的可同时检测CC和HQ的方法包括高效液相色谱法[4]、毛细管电泳法[5]、分光光度法[6]和化学发光法[7]等。这些方法通常需要昂贵的仪器和复杂的操作流程。电化学分析方法具有检测快速、仪器简单、便于现场测试、选择性高和灵敏度高等特点[8-9],而CC和HQ具有较高的电化学活性,电化学分析方法也是CC和HQ检测的有效方法。电化学方法同时检测CC和HQ的难点在于二者的峰电势接近,信号峰易发生重叠,并且二者在电极表面的竞争过程可能引起峰电流与浓度的关系偏离线性[10]。因此,对电极进行化学修饰以获得足够大的峰电势差以及良好的峰电流和浓度的线性关系在电化学同时检测CC和HQ的研究中具有重要意义。目前,已有多种复合或杂化纳米材料被用于邻、对苯二酚的同时电化学检测,例如金纳米粒子与氧化石墨烯复合物、聚嘧啶与石墨烯复合物、氧化镍与碳纳米管复合物、三维花状硫化铜纳米片修饰的碳纳米碎片等[11-14]。这些材料能够区分并放大邻苯二酚和对苯二酚的峰信号,但是存在合成过程复杂、成本高的问题。

    金属氧化物纳米粒子具有高活性、特殊的电子性质、高比表面积以及独特的光电性质等特点,是重要的无机材料[15-16]。纳米氧化铜(CuO(NP))是p型半导体金属氧化物,在多相催化、气体传感器、锂离子电池和电化学传感等诸多领域被广泛研究[17-20]。CuO(NP)可采用微波辐射、激光烧蚀、声化学分解、快速液相沉淀等方法合成[21-24]。

    CuO(NP)作为传感材料,具有良好的电化学活性和稳定性。以CuO(NP)为基础的电化学传感器通常需要结合其他材料,以达到提高导电性和避免纳米颗粒聚集的目的[25]。碳纳米管具有良好的导电性、化学稳定性和生物相容性,作为优良的电极修饰材料,在多种样品的检测领域被广泛应用[26-28]。本文将商品化CuO(NP)和羧化多壁碳纳米管(MCT)复合物作为修饰玻碳电极(GCE)的修饰材料,所制备的CuO(NP)-MCT/GCE电极结合了两种材料区分CC和HQ电信号以及放大氧化还原峰电流的优势,获得较高响应电流的同时对两种同分异构体表现出优良的识别能力,二者的氧化还原峰电势有显著差别(图 1)。以此建立了成本低廉、简便、快速的可同时检测CC和HQ的电化学传感方法。

    图 1

    图 1.  CuO(NP)-CNT/GCE制备过程示意图
    Figure 1.  Schematic diagram for the preparation of CuO(NP)-CNT/GCE

    羧化多壁碳纳米管(MCT,纯度>95%,内径ϕ:5~15 nm,外径Φ>50 nm,长度:10~20 μm)和CuO(NP)(d=40 nm)购自阿拉丁试剂有限公司;CC、HQ、二水合磷酸二氢钠、十二水合磷酸氢二钠、N, N-二甲基甲酰胺(DMF)、无水乙醇、氯化钾均为分析纯试剂,购自成都科隆化学品公司;实验用水均为超纯水。所有试剂未经纯化直接使用。

    CHI 760e型电化学工作站(上海辰华公司);pHS-320型酸度计(成都世纪方舟有限公司);KQ-100E型超声波清洗仪(苏州昆山舒美超声仪器有限公司);三电极体系:玻碳电极(GCE)、纳米氧化铜(CuO(NP))或MCT修饰的GCE为工作电极,参比和对电极分别为Ag/AgCl(3 mol/L KCl)电极和铂丝电极(上海辰华公司)。

    1.2.1   CuO(NP)-MCT/GCE的制备

    将CuO(NP)和MCT置于DMF中,超声分散20 min,得到CuO(NP)质量浓度为10 mg/mL、MCT质量浓度为2 mg/mL的悬浮液,每次使用前超声10 min。GCE电极(有效直径3 mm)用0.05 μm氧化铝粉末及麂皮抛光至镜面,然后依次在无水乙醇和超纯水中超声1 min后,在红外灯下烘干。用微量移液器分别移取9 μL CuO(NP)-MCT悬浮液滴加至GCE电极表面,然后在红外灯下烘干,即制得CuO(NP)-MCT/GCE电极。修饰量优化部分,向GCE电极表面滴加CuO(NP)-MCT悬浮液的体积以此为3、4、5、6、7、8和9 μL。CuO(NP)和MCT比例的影响研究部分,MCT质量浓度为2 mg/mL,CuO(NP)质量浓度分别为2、5、10、15和20 mg/mL。

    1.2.2   电化学测量

    向含有CC和HQ的磷酸缓冲溶液(PBS,0.1 mol/L,pH=7.4)中通入高纯N2气10 min,然后以CuO(NP)-MCT/GCE为工作电极进行循环伏安扫描或微分脉冲伏安扫描。pH优化研究,分别在pH=4.3、5.1、6.1、7.4、8.1的含有0.500 mmol/L CC和HQ的PBS中进行。扫描电势范围为-0.1~0.6 V,循环伏安法扫速为50 mV/s,研究峰电流与扫速关系时的扫速分别为10、20、30、40、50、60、70、80、90、100、125、150、175、200 mV/s;脉冲伏安法扫描电势增量为4 mV,脉冲幅度为0.1 V,脉冲宽度为0.05 s。

    采用循环伏安法研究了CC和HQ共存时在GCE和CuO(NP)、CNT单独修饰的GCE以及CuO(NP)-CNT复合物修饰的GCE这3种修饰电极上的电化学行为,结果如图 2所示。在未修饰的GCE上,CC和HQ的氧化峰重叠。在CuO(NP)/GCE上,二者的氧化峰依然重叠,但是氧化峰向低电势移动,峰电流增大。在MCT/GCE上,CC和HQ的信号峰未发生重叠,氧化峰均向低电势移动,还原峰略向高电势移动,并且氧化还原峰电流显著增加。在CuO(NP)-MCT/GCE上,CC的氧化峰和还原峰电势分别为189和138 mV;HQ的氧化峰和还原峰电势分别为76和23 mV。CC和HQ的氧化还原峰电势差与MCT修饰电极一致,氧化峰电势差为113 mV,还原峰电势差为115 mV;不同的是氧化峰电势略向高电势移动;并且CC氧化峰电流增加至MCT/GCE上的1.8倍,HQ氧化峰电流至1.4倍,峰电流显著增加。说明CuO(NP)-MCT复合物结合了两种纳米材料的优势,对CC和HQ具有更强的催化作用,CuO(NP)-MCT可用于对CC和HQ的同时检测。

    图 2

    图 2.  GCE(a)、CuO(NP)/GCE(b)、MCT/GCE(c)和CuO(NP)-MCT/GCE(d)在CC和HQ溶液中的循环伏安图
    Figure 2.  The cyclic voltammograms at GCE(a), CuO(NP)/GCE(b), MCT/GCE(c) and CuO(NP)-MCT/GCE(d) in CC and HQ solution

    c(CC)=c(HQ)=0.500 mmol/L, supporting electrolyte:PBS(pH=7.4); scan rate:50 mV/s

    CuO(NP)-MCT复合物中两种材料的比例对CC和HQ的峰电流有显著影响,含有2 mg/mL MCT和不同浓度CuO(NP)的悬浮液修饰的GCE在CC和HQ溶液中的循环伏安曲线如图 3所示。CuO(NP)浓度从2 mg/mL增大至10 mg/mL,两种酚的氧化还原峰电流均随之增大。但是继续增大CuO(NP)浓度,峰电流则降低,这可能是由于CuO(NP)比例过高,阻碍了MCT的电子传输过程。因此,选择CuO(NP)浓度为10 mg/mL,既CuO(NP)与MCT质量比为5:1的悬浮液作为修饰液。

    图 3

    图 3.  MCT和不同浓度CuO(NP)修饰的GCE在CC和HQ溶液中的循环伏安图
    Figure 3.  The cyclic voltammograms at CuO(NP)-CNT/GCE prepared with different concentrations of CuO(NP) in CC and HQ solution

    c(CC)=c(HQ)=0.500 mmol/L, supporting electrolyte:PBS(pH=7.4); scan rate:50 mV/s

    研究了GCE表面CuO(NP)-MCT修饰量修对CC和HQ循环伏安扫描结果的影响(图 4A)。分别用3~9 μL CuO(NP)-MCT悬浮液修饰GCE,随修饰量增大,两种酚的氧化还原峰电流均增大。但是继续增大修饰体积存在修饰液易溢出玻碳表面和修饰层过厚易脱落的问题,所以选择9 μL CuO(NP)-MCT悬浮液修饰的GCE进行CC和HQ的同时测定。

    图 4

    图 4.  (A) 不同体积CuO(NP)-MCT悬浮液修饰的GCE在CC和HQ溶液中的循环伏安图,(B)CuO(NP)-MCT/GCE在不同pH的CC和HQ溶液中的循环伏安曲线
    Figure 4.  (A)The cyclic voltammograms of GCEs modified by different volumes of CuO(NP)-MCT in the solution of CC and HQ; (B)The cyclic voltammograms of CuO(NP)-MCT/GCE in PBS containing CC and HQ with different pH

    A:The volumes of CuO(NP)-MCT on the GCEs surface are 3, 4, 5, 6, 7, 8, and 9 μL separately for line a to g

    CC和HQ被氧化的过程中失去两个电子,产生两个H+[29],支持电解质溶液pH对氧化还原过程有重要影响,因此研究了pH对CuO(NP)-MCT/GCE上CC和HQ电化学行为的影响(图 4B)。在4.3~8.1范围内,随着pH值从4.3升至8.1,CC和HQ的氧化还原峰均向负电势移动,峰电流大小随pH变化无明显变化规律,与弱酸性和弱碱性条件相比,pH=7.4时峰电流稍高,因此选择pH=7.4的PBS作为测定CC和HQ的支持电解质溶液。

    图 5是不同扫速条件下CuO(NP)-MCT/GCE在CC和HQ溶液中的循环伏安图。随扫速增加,氧化峰向正电势移动,还原峰电势向负电势移动,说明在该电极上CC和HQ的氧化还原反应是准可逆过程(图 5A)。另外,随扫速增加,峰电流增大,在10~200 mV/s范围内CC和HQ的氧化峰电流Ipa和还原峰电流Ipc均与扫速的平方根成正比(图 5B),相关系数均高于0.999,说明CC和HQ在CuO(NP)-MCT/GCE的电化学过程由扩散过程控制。

    图 5

    图 5.  (A) 不同扫速下CuO(NP)-MCT/GCE在CC和HQ溶液中的循环伏安图;(B)CC和HQ的氧化峰电流、还原峰电流与扫速平方根的线性关系曲线
    Figure 5.  (A)The cyclic voltammograms of CuO(NP)-MCT/GCE at different scan rates. (B)The relationship curves of anodic and cathodic peak currents vs square root of scan rates

    A:from a to n:10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 125, 150, 175, 200 mV/s

    在优化的CuO(NP)-MCT比例、修饰量和pH条件下,用CuO(NP)-MCT/GCE对不同浓度的CC和HQ进行了微分脉冲伏安法检测。结果显示,在6.0×10-7~3.0×10-3 mol/L浓度范围内,CC和HQ的峰电流Ip与浓度呈线性关系(图 6)。线性回归方程分别为Ip(CC)=128+112c和Ip(HQ)=14.6+78.9c,相关系数依次为0.999和0.998,检出限(S/N=3)依次为1.0×10-7和1.6×10-7 mol/L。与同类同时测定CC和HQ的电极相比,CuO(NP)-MCT/GCE具有检出限低,线性范围宽的特点(表 1)。

    图 6

    图 6.  CuO(NP)-MCT/GCE在不同浓度CC和HQ溶液中的微分脉冲伏安曲线
    Figure 6.  The differential pulse voltammetric determination with CuO(NP)-MCT/GCE in solutions containing different concentrations of CC and HQ. (The inset is the linear relationship curves between peak currents and concentrations)

    From a to i: 0, 0.000600, 0.00100, 0.0100, 0.100, 0.300, 0.500, 1.00, 3.00 mmol/L

    表 1

    表 1  不同修饰电极同时测定CC和HQ的比较
    Table 1.  Comparison of different electrochemical sensors for the detection of CC and HQ
    下载: 导出CSV
    Modified electrode Linear range/(μmol·L-1) Detection limit/(μmol·L-1) Reference
    CC HQ CC HQ
    Graphitic Carbon Nitride Nanosheets-CNT/GCE 1~200 1~250 0.09 0.13 [30]
    Reduced graphene oxide-MCT/GCE 5.5~540 8~391 1.8 2.6 [31]
    AgNPs/MCT/GCE 20~260 2.5~260 0.2 0.16 [32]
    MCT@Reduced Graphene Oxide Nanoribbon/GCE 15~1101 15~921 1.73 3.89 [9]
    NiO/Carbon nanotubes/GCE 10~400 10~500 2.5 2.5 [13]
    Graphene oxide/AuNPs/GCE 20~1000 20~1000 0.4 0.1 [11]
    Graphene/GCE 80~1000 80~1000 0.5 0.1 [33]
    CuO(NP)-MCT/GCE 0.6~3000 0.6~3000 0.1 0.16 This work

    对以CuO(NP)-MCT修饰电极作为工作电极检测CC和HQ的电化学方法的稳定性和重现性进行了考察。使用该电极对0.500 mmol/L的CC和HQ的混合溶液连续测定10次,峰电流的相对标准偏差RSD依次为3.5%和3.1%,说明该检测方法具有较好的稳定性。用同样的方法分别制备了6根CuO(NP)-MCT/GCE,测定0.500 mmol/L的CC和HQ溶液,RSD分别为3.4%和3.8%。这表明该修饰电极制备方法具有较好的重现性。

    以CuO(NP)-MCT/GCE为工作电极,在优化的实验条件下,采用脉冲伏安扫描法对自来水样和西南民族大学映月潭水样进行了检测,未产生CC和HQ信号。对水样进行了加标回收检测,结果如表 2所示,CC和HQ的加标回收率在94.6%~101.1%范围内。

    表 2

    表 2  水样中CC和HQ加标回收实验结果
    Table 2.  Results of recovery experiments on water samples
    下载: 导出CSV
    Sample Added/(mmol·L-1) Found/(mmol·L-1) Recovery/% Added/(mmol·L-1) Found/(mmol·L-1) Recovery/%
    Tap water CC 0.050 0 0.047 3 94.6 1.00 0.972 97.2
    HQ 0.050 0 0.050 6 101.2 1.00 1.011 101.1
    Yingyuetan lake water CC 0.050 0 0.048 2 96.4 1.00 1.006 100.6
    HQ 0.050 0 0.047 9 95.8 1.00 0.967 96.7

    本研究以纳米氧化铜(CuO(NP))和羧化多壁碳纳米管(MCT)复合物修饰玻碳电极,性质相近的同分异构体邻苯二酚(CC)和对苯二酚(HQ)在该电极表面的氧化峰电势差和还原峰电势差均超过110 mV,足以区分两者信号。该修饰电极与单一材料修饰电极相比,结合了CuO(NP)放大电信号和MCT强电催化性能的优势,CC和HQ具有更高的峰电流。CuO(NP)与MCT的浓度比例对电流放大程度有重要影响,二者质量比为5:1时,CC和HQ的峰电流最高。对复合物修饰量以及支持电解质pH液进行了优化。在优化的条件下,CC和HQ的峰电流与浓度均在6.0×10-7~3.0×10-3 mol/L范围内呈良好的线性关系,检出限(S/N=3)分别为1.0×10-7和1.6×10-7 mol/L。为考察该电极在实际水样中的检测效果,对自来水样和映月潭水样进行了加标回收检测,回收率在合理范围内。本文中CuO(NP)-MCT/GCE的构建过程具有成本低、操作简便、快速的特点,在水样中CC和HQ的同时检测中具有较好应用前景。


    1. [1]

      Wang H F, Wu Y Y, Yan X P. Room-Temperature Phosphorescent Discrimination of Catechol from Resorcinol and Hydroquinone Based on Sodium Tripolyphosphate Capped Mn-Doped ZnS Quantum Dots[J]. Anal Chem, 2013, 85(3):  1920-1925.

    2. [2]

      Chen T T, Xu J Q, Arsalan M. Controlled Synthesis of Au@Pd Core-Shell Nanocomposites and their Application for Electrochemical Sensing of Hydroquinone[J]. Talanta, 2019, 198:  78-85.

    3. [3]

      Huang D L, Wang J, Cheng F. Synergistic Effect of a Cobalt Fluoroporphyrin and Graphene Oxide on the Simultaneous Voltammetric Determination of Catechol and Hydroquinone[J]. Microchim Acta, 2019, 186(6):  1-11.

    4. [4]

      Marrubini G, Calleri E, Coccini T. Direct Analysis of Phenol, Catechol and Hydroquinone in Human Urine by Coupled-Column HPLC with Fluorimetric Detection[J]. Chromatographia, 2005, 62(1/2):  25-31.

    5. [5]

      Xie T Y, Liu Q W, Shi Y R. Simultaneous Determination of Positional Isomers of Benzenediols by Capillary Zone Electrophoresis with Square Wave Amperometric detection[J]. J Chromatogr A, 2006, 1109(2):  317-321.

    6. [6]

      Liu J, Lin Z. Simultaneous Determination of Mixed Phenol, Catechol, and Quinol by Double Fourier Transform Filtering and Second Ratio Spectra Derivative Spectrophotometry[J]. Spectrosc Spectr Anal, 2000, 20(4):  480-483.

    7. [7]

      Cui H, Zhang Q L, Myint A. Chemiluminescence of Cerium(IV)-Rhodamine 6G-Phenolic Compound System[J]. J Photochem Photobiol A, 2006, 181(2/3):  238-245.

    8. [8]

      Chen T W, Yu X N, Li S J. Simultaneous Determination of Dihydroxybenzene Isomers Using Glass Carbon Electrode Modified with 3D CNT-Graphene Decorated with Au Nanoparticles[J]. Int J Electrochem Sc, 2019, 14(8):  7037-7046.

    9. [9]

      Yang S Y, Yang M, Liu Q Y. An Ultrasensitive Electrochemical Sensor Based on Multiwalled Carbon Nanotube@Reduced Graphene Oxide Nanoribbon Composite for Simultaneous Determination of Hydroquinone, Catechol and Resorcinol[J]. J Electrochem Soc, 2019, 166(6):  B547-B553.

    10. [10]

      Zhao C, Song J F, Zhang J C. Determination of Total Phenols in Environmental Wastewater by Flow-Injection Analysis with a Biamperometric Detector[J]. Anal Bioanal Chem, 2002, 374(3):  498-504.

    11. [11]

      王中腾, 刘寒寒, 滕辉. 石墨烯/纳米金复合修饰电极对邻苯二酚和对苯二酚的同时测定[J]. 安徽科技学院学报, 2018,32,(5): 64-72. WANG Zhongteng, LIU Hanhan, TENG Hui. A Voltammetric Sensor Based on Graphene-Gold Nanocomposite Film for Simultaneous Determination of Hydroquinone and Catechol[J]. J Anhui Sci Tech Univ, 2018, 32(5):  64-72.

    12. [12]

      付菊, 谭小红, 宋新建. 聚嘧啶/石墨烯复合膜修饰电极的制备及其用于邻苯二酚和对苯二酚的同时检测[J]. 湖北民族学院学报(自然科学版), 2016,34,(2): 195-198. FU Ju, TAN Xiaohong, SONG Xinjian. Polypyrimidine/Graphene Composite Film Modified Electrode for the Simultaneous Detection of Catechol and Hydroquinone[J]. J Hubei Univ Nationnalities(Nat Sci Edn), 2016, 34(2):  195-198.

    13. [13]

      Zhao L, Yu J, Yue S Z. Nickel Oxide/Carbon Nanotube Nanocomposites Prepared by Atomic Layer Deposition for Electrochemical Sensing of Hydroquinone and Catechol[J]. J Electroanal Chem, 2018, 808:  245-251.

    14. [14]

      Alshahrani L A, Miao L Q, Zhang Y Y. 3D-Flower-Like Copper Sulfide Nanoflake-Decorated Carbon Nanofragments-Modified Glassy Carbon Electrodes for Simultaneous Electrocatalytic Sensing of Coexisting Hydroquinone and Catechol[J]. Sensors, 2019, 19(10):  1-12.

    15. [15]

      Bozkurt G, Bayrakceken A, Ozer A K. Synthesis and Characterization of CuO at Nanoscale[J]. Appl Surf Sci, 2014, 318:  244-250.

    16. [16]

      Khanna P K, Gaikwad S, Adhyapak R. Synthesis and Characterization of Copper Nanoparticles[J]. Mater Lett, 2007, 61(25):  4711-4714.

    17. [17]

      Teng F, Yao W Q, Zheng Y F. Synthesis of Flower-like CuO Nanostructures as a Sensitive Sensor for Catalysis[J]. Sens Actuators B, 2008, 134(2):  761-768.

    18. [18]

      Patil S A, Patil L A, Patil D R. CuO-Modified Tin Titanate Thick Film Resistors as H2-Gas Sensors[J]. Sens Actuators B, 2007, 123(1):  233-239.

    19. [19]

      Xiang J Y, Tu J P, Huang X H. A Comparison of Anodically Grown CuO Nanotube Film and Cu2O Film as Anodes for Lithium Ion Batteries[J]. J Solid State Electrochem, 2008, 12(7/8):  941-945.

    20. [20]

      Alizadeh T, Mirzagholipur S. A Nafion-Free Non-Enzymatic Amperometric Glucose Sensor Based on Copper Oxide Nanoparticles-Graphene Nanocomposite[J]. Sens Actuators B, 2014, 198:  438-447.

    21. [21]

      Wang H, Xu J Z, Zhu J J. Preparation of CuO Nanoparticles by Microwave Irradiation[J]. J Cryst Growth, 2002, 244(1):  88-94.

    22. [22]

      Suzuki K, Tanaka N, Ando A. Size-Selected Copper Oxide Nanoparticles Synthesized by Laser Ablation[J]. J Nanopart Res, 2012, 14(5):  1-11.

    23. [23]

      Kumar R V, Diamant Y, Gedanken A. Sonochemical Synthesis and Characterization of Nanometer-Size Transition Metal Oxides from Metal Acetates[J]. Chem Mater, 2000, 12(8):  2301-2305.

    24. [24]

      Zhu J W, Li D, Chen H Q. Highly Dispersed CuO Nanoparticles Prepared by a Novel Quick-Precipitation Method[J]. Mater Lett, 2004, 58(26):  3324-3327.

    25. [25]

      Arvand M, Ardaki M S, Zanjanchi M A. A New Sensing Platform Based on Electrospun Copper Oxide/Ionic Liquid Nanocomposite for Selective Determination of Risperidone[J]. RSC Adv, 2015, 5(51):  40578-40587.

    26. [26]

      罗云凤, 刘保双, 李春香. 基于碳纳米管/Ag/MoS2转导层的全固态钙离子选择电极[J]. 应用化学, 2019,36,(6): 704-710. LUO Yunfeng, LIU Baoshuang, LI Chunxiang. All Solid-State Calcium Ion Selective Electrode Based on Carbon Nanotube/Ag/MoS2 Transducer[J]. Chinese J Appl Chem, 2019, 36(6):  704-710.

    27. [27]

      徐思远, 雷平, 晋冠平. 三聚氰胺基螯合树脂/碳纳米管修饰充蜡石墨电极阳极溶出伏安法测定铅和镉[J]. 应用化学, 2014,31,(2): 206-211. XU Siyuan, LEI Ping, JIN Guanping. Determination of Pb(Ⅱ), Cd(Ⅱ) with Melamine Chelating Resin/Multi-walled Carbon Nanotubes Composites Modified Waxed Graphite Electrode[J]. Chinese J Appl Chem, 2014, 31(2):  206-211.

    28. [28]

      于浩, 郑笑晨, 刘冉彤. 多壁碳纳米管负载铁氰化铜-铁修饰电极的制备及对亚硝酸根的测定[J]. 应用化学, 2014,31,(11): 1336-1344. YU Hao, ZHENG Xiaochen, LIU Rantong. Preparation of Copper-iron Hexacyanoferrate Loaded Multi-walled Carbon Nanotubes Modified Electrode for the Determination of Nitrite[J]. Chinese J Appl Chem, 2014, 31(11):  1336-1344.

    29. [29]

      孟奎奎, 郭珈玲, 云阳方. 邻苯二酚和对苯二酚在金纳米修饰玻碳电极(GNP/GCE)上的同时灵敏检测[J]. 化学研究与应用, 2018,30,(3): 432-436. MENG Kuikui, CUO Jialing, YUN Yangfang. Simultaneous Sensitive Determination of Catechol and Hydroquinone at Gold Nanoparticles Modified Glassy Carbon Electrode[J]. Chem Res Appl, 2018, 30(3):  432-436.

    30. [30]

      Zhang H Q, Huang Y H, Hu S R. Self-assembly of Graphitic Carbon Nitride Nanosheets-Carbon Nanotube Composite for Electrochemical Simultaneous Determination of Catechol and Hydroquinone[J]. Electrochim Acta, 2015, 176:  28-35.

    31. [31]

      Hu F X, Chen S H, Wang C Y. Study on the Application of Reduced Graphene Oxide and Multiwall Carbon Nanotubes Hybrid Materials for Simultaneous Determination of Catechol, Hydroquinone, p-Cresol and Nitrite[J]. Anal Chim Acta, 2012, 724:  40-46.

    32. [32]

      Goulart L A, Goncalves R, Correa A A. Synergic Effect of Silver Nanoparticles and Carbon Nanotubes on the Simultaneous Voltammetric Determination of Hydroquinone, Catechol, Bisphenol A and Phenol[J]. Microchim Acta, 2017, 185(1):  1-9.

    33. [33]

      万其进, 廖华玲, 刘义. 石墨烯修饰电极同时测定邻苯二酚和对苯二酚[J]. 武汉工程大学学报, 2013,35,(2): 16-23. WAN Qijin, LIAO Hualing, LIU Yi. Simultaneous Determination of Catechol and Hydroquinpne in Graphene Modified Electrode[J]. J Wuhan Inst Tech, 2013, 35(2):  16-23.

  • 图 1  CuO(NP)-CNT/GCE制备过程示意图

    Figure 1  Schematic diagram for the preparation of CuO(NP)-CNT/GCE

    图 2  GCE(a)、CuO(NP)/GCE(b)、MCT/GCE(c)和CuO(NP)-MCT/GCE(d)在CC和HQ溶液中的循环伏安图

    Figure 2  The cyclic voltammograms at GCE(a), CuO(NP)/GCE(b), MCT/GCE(c) and CuO(NP)-MCT/GCE(d) in CC and HQ solution

    c(CC)=c(HQ)=0.500 mmol/L, supporting electrolyte:PBS(pH=7.4); scan rate:50 mV/s

    图 3  MCT和不同浓度CuO(NP)修饰的GCE在CC和HQ溶液中的循环伏安图

    Figure 3  The cyclic voltammograms at CuO(NP)-CNT/GCE prepared with different concentrations of CuO(NP) in CC and HQ solution

    c(CC)=c(HQ)=0.500 mmol/L, supporting electrolyte:PBS(pH=7.4); scan rate:50 mV/s

    图 4  (A) 不同体积CuO(NP)-MCT悬浮液修饰的GCE在CC和HQ溶液中的循环伏安图,(B)CuO(NP)-MCT/GCE在不同pH的CC和HQ溶液中的循环伏安曲线

    Figure 4  (A)The cyclic voltammograms of GCEs modified by different volumes of CuO(NP)-MCT in the solution of CC and HQ; (B)The cyclic voltammograms of CuO(NP)-MCT/GCE in PBS containing CC and HQ with different pH

    A:The volumes of CuO(NP)-MCT on the GCEs surface are 3, 4, 5, 6, 7, 8, and 9 μL separately for line a to g

    图 5  (A) 不同扫速下CuO(NP)-MCT/GCE在CC和HQ溶液中的循环伏安图;(B)CC和HQ的氧化峰电流、还原峰电流与扫速平方根的线性关系曲线

    Figure 5  (A)The cyclic voltammograms of CuO(NP)-MCT/GCE at different scan rates. (B)The relationship curves of anodic and cathodic peak currents vs square root of scan rates

    A:from a to n:10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 125, 150, 175, 200 mV/s

    图 6  CuO(NP)-MCT/GCE在不同浓度CC和HQ溶液中的微分脉冲伏安曲线

    Figure 6  The differential pulse voltammetric determination with CuO(NP)-MCT/GCE in solutions containing different concentrations of CC and HQ. (The inset is the linear relationship curves between peak currents and concentrations)

    From a to i: 0, 0.000600, 0.00100, 0.0100, 0.100, 0.300, 0.500, 1.00, 3.00 mmol/L

    表 1  不同修饰电极同时测定CC和HQ的比较

    Table 1.  Comparison of different electrochemical sensors for the detection of CC and HQ

    Modified electrode Linear range/(μmol·L-1) Detection limit/(μmol·L-1) Reference
    CC HQ CC HQ
    Graphitic Carbon Nitride Nanosheets-CNT/GCE 1~200 1~250 0.09 0.13 [30]
    Reduced graphene oxide-MCT/GCE 5.5~540 8~391 1.8 2.6 [31]
    AgNPs/MCT/GCE 20~260 2.5~260 0.2 0.16 [32]
    MCT@Reduced Graphene Oxide Nanoribbon/GCE 15~1101 15~921 1.73 3.89 [9]
    NiO/Carbon nanotubes/GCE 10~400 10~500 2.5 2.5 [13]
    Graphene oxide/AuNPs/GCE 20~1000 20~1000 0.4 0.1 [11]
    Graphene/GCE 80~1000 80~1000 0.5 0.1 [33]
    CuO(NP)-MCT/GCE 0.6~3000 0.6~3000 0.1 0.16 This work
    下载: 导出CSV

    表 2  水样中CC和HQ加标回收实验结果

    Table 2.  Results of recovery experiments on water samples

    Sample Added/(mmol·L-1) Found/(mmol·L-1) Recovery/% Added/(mmol·L-1) Found/(mmol·L-1) Recovery/%
    Tap water CC 0.050 0 0.047 3 94.6 1.00 0.972 97.2
    HQ 0.050 0 0.050 6 101.2 1.00 1.011 101.1
    Yingyuetan lake water CC 0.050 0 0.048 2 96.4 1.00 1.006 100.6
    HQ 0.050 0 0.047 9 95.8 1.00 0.967 96.7
    下载: 导出CSV
  • 加载中
计量
  • PDF下载量:  7
  • 文章访问数:  2246
  • HTML全文浏览量:  652
文章相关
  • 发布日期:  2020-10-01
  • 收稿日期:  2020-02-21
  • 接受日期:  2020-05-09
  • 修回日期:  2020-03-18
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

/

返回文章